Abiurana vs Gangaw
Pouteria guianensis against Mesua ferrea. Every number below names the publication it came from.
| Property | Abiurana | Gangaw |
|---|---|---|
| Janka hardness | 2,921 lbfLPF/SFB Madeiras Brasileiras | 2,890 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 58.7 lb/ft³LPF/SFB Madeiras Brasileiras | 63.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 20,382 lb/in²LPF/SFB Madeiras Brasileiras | 24,065 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | — | 2.87 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 9,871 lb/in²LPF/SFB Madeiras Brasileiras | 12,430 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 13.3%LPF/SFB Madeiras Brasileiras | 15.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.76LPF/SFB Madeiras Brasileiras | 1.58Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Gangaw carries 18% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.