Janka hardness chart

The Janka test presses a steel ball of 11.28 mm diameter into the wood to half its diameter. The force needed is the Janka number. It measures resistance to denting, and it does not measure stiffness or strength.

571 of 1785 species carry a published laboratory test. A further 1212 carry a value estimated from density; those estimates are excluded from this chart. Use the toggle in the header to change the unit.

#WoodJanka (lbf)
1Lignumvitae4,500 lbf
2UrucuranaSloanea sp.4,206 lbf
3UrucuranaSloanea nitida4,057 lbf
4Miraúba4,032 lbf
5Curupay3,840 lbf
6Jatobá / jutaí-do-campo3,792 lbf
7Wamara3,692 lbf
8Ipe3,680 lbf
9Jataipeba3,650 lbf
10Marishballi3,570 lbf
11Jarana3,500 lbf
12Manbarklak3,480 lbf
13Muirapixuna3,435 lbf
14Cumaru3,415 lbf
15RosadinhoPeltogyne paniculata3,386 lbf
16Casca-preciosa3,369 lbf
17Azobe3,350 lbf
18Maria-preta3,331 lbf
19Caraiperana3,294 lbf
20Pau-santo3,261 lbf
21MaçarandubaManilkara sp.3,228 lbf
22African ebony3,220 lbf
23Castanha-de-cutiaCouepia robusta3,206 lbf
24Casuarina3,200 lbf
25Bulletwood3,190 lbf
26Angelim / angelim-rajado3,177 lbf
27Indian rosewoodDalbergia latifolia3,170 lbf
28Pracuúba-da-terra-firme3,159 lbf
29Macucu-branco3,153 lbf
30Macawood3,150 lbf
31Cachaporra-do-gentio3,139 lbf
32IpêHandroanthus serratifolius = Tabebuia serratifolia3,100 lbf
33Sapucaia3,100 lbf
34Brush Box3,088 lbf
35Cabreúva-parda3,075 lbf
36IngáInga paraensis3,064 lbf
37MaçarandubaManilkara huberi3,047 lbf
38Angelim-vermelho3,045 lbf
39MururéBrosimum gaudichaudii3,036 lbf
40Belian3,020 lbf
41Rhodesian-Teak2,990 lbf
42Muhimbi2,975 lbf
43Aromata2,960 lbf
44AbiuranaPouteria egregia2,950 lbf
45Uxirana2,948 lbf
46Abiurana-seca2,945 lbf
47Angico2,941 lbf
48Missanda2,930 lbf
49TuturubáPouteria oblanceolata2,923 lbf
50AbiuranaPouteria guianensis2,921 lbf
51SucupiraBowdichia nitida2,903 lbf
52Kaneelhart2,900 lbf
53Gangaw2,890 lbf
54IngáInga sp2,846 lbf
55Sapucaia / sapucaia-vermelha2,831 lbf
56West Indian Lancewood2,830 lbf
57TanimbucaBuchenavia sp2,829 lbf
58Okan2,780 lbf
59Mangle Colorado2,760 lbf
60Caraipé2,754 lbf
61Turpentine2,750 lbf
62East African Olive2,740 lbf
63Kamassi2,730 lbf
64Maçarandubarana2,725 lbf
65Brazilian rosewood2,720 lbf
66Black Cabbage-Bark2,700 lbf
67Leche Perra2,700 lbf
68Castanha-de-cutiaAcioa edulis2,696 lbf
69Barrote2,693 lbf
70Bubinga2,690 lbf
71Anoerá-ferro2,683 lbf
72Goiabão2,646 lbf
73Abiurana-brancaPouteria caimito2,608 lbf
74East Indian Satinwood2,600 lbf
75Mecrusse2,540 lbf
76Parinari / bafo-de-boi-mirim2,522 lbf
77Pau-branco2,518 lbf
78Cuiarana2,513 lbf
79Canafístula2,500 lbf
80Oak2,500 lbf
81AbiuranaPouteria anomala2,472 lbf
82Muwa2,470 lbf
83UrucuranaSwartzia recurva2,469 lbf
84MatamatáEschweilera coriacea2,467 lbf
85AbiuranaPouteria sp2,418 lbf
86MatamatáEschweilera pedicellata = Eschweilera longipes2,410 lbf
87TuturubáPouteria gongrijpii = Franchetella gongrijpii2,396 lbf
88Amora / amoreira2,385 lbf
89FusticChlorophora tinctoria2,380 lbf
90Demerara Greenheart2,360 lbf
91Courbaril2,350 lbf
92Greenheart2,350 lbf
93Fava-orelha-de-negro2,346 lbf
94Matamatá / sapucaia-amargosa2,341 lbf
95Uxi2,335 lbf
96BreuProtium sp.2,317 lbf
97Mora2,300 lbf
98Burma Lancewood2,270 lbf
99Pyinkado2,248 lbf
100Carne D'Anta2,240 lbf
101TanimbucaTerminalia amazonia2,235 lbf
102Indian Laurel2,220 lbf
103Balsamo2,200 lbf
104Canalete2,200 lbf
105Taniboca2,191 lbf
106Muhuhu2,190 lbf
107Essia2,180 lbf
108Faveira-amargosaVatairea paraensis2,174 lbf
109Burma Padauk2,170 lbf
110Breu-manga2,169 lbf
111Louro-faia2,169 lbf
112Pau-amarelo2,168 lbf
113Angelim-amargoso2,167 lbf
114MandioqueiraQualea brevipedicellata2,165 lbf
115Goncalo alves2,160 lbf
116Danta2,140 lbf
117Pignut hickory2,140 lbf
118SucupiraDiplotropis purpurea2,140 lbf
119Chengal2,130 lbf
120Tembusu2,120 lbf
121Ohia2,090 lbf
122Conduru / pau-vermelho2,062 lbf
123Bluegum2,060 lbf
124Janitá2,059 lbf
125Pau-jacaré2,053 lbf
126Muiracatiara-rajada2,051 lbf
127African Homalium2,050 lbf
128Karri2,040 lbf
129Wallaba2,040 lbf
130Louro-amarelo2,019 lbf
131MatamatáEschweilera grandiflora = Eschweilera cf fracta1,995 lbf
132Angelim-tinto1,989 lbf
133Cupiúba1,989 lbf
134Mockernut hickory1,970 lbf
135Sali1,970 lbf
136Taxi-preto / taxiarana1,962 lbf
137Degame1,940 lbf
138Seringarana1,925 lbf
139Jarrah1,910 lbf
140Chupón1,880 lbf
141Shagbark hickory1,880 lbf
142Garapa1,863 lbf
143Mueri1,860 lbf
144Purpleheart1,860 lbf
145Ranggu1,860 lbf
146Nargusta1,855 lbf
147Peroba1,852 lbf
148Burada1,830 lbf
149Mtundu1,830 lbf
150Pecan hickory1,820 lbf
151Afzelia1,810 lbf
152Brown Sterculia1,810 lbf
153Shellbark hickory1,810 lbf
154Andira-uxi1,788 lbf
155Abiurana-mangabarana1,781 lbf
156Shorea1,780 lbf
157Nkobakoba1,770 lbf
158Açoita-cavalo1,767 lbf
159Araracanga1,757 lbf
160Angelin1,750 lbf
161Benge1,750 lbf
162Black WattleAcacia mollissima1,750 lbf
163Maragonçalo1,746 lbf
164Embira-de-preguiça1,731 lbf
165Peroba rosa1,730 lbf
166Para-angelim1,720 lbf
167Piquia1,720 lbf
168Rengas1,720 lbf
169RosadinhoMicropholis venulosa1,720 lbf
170Kempas1,710 lbf
171Black locust1,700 lbf
172Pilon1,700 lbf
173Suradan1,700 lbf
174TentoOrmosia paraensis1,688 lbf
175Muiracatiara1,684 lbf
176Sandalwood1,680 lbf
177Glícia1,671 lbf
178African Celtis1,670 lbf
179RosadinhoPiptadenia gonoacantha = Piptadenia communis1,669 lbf
180Tatajuba1,660 lbf
181Angelim-pedraHymenolobium modestum1,647 lbf
182Pequiarana1,642 lbf
183TanimbucaBuchenavia tetraphylla = Buchenavia capitata1,640 lbf
184Andaman Padauk1,630 lbf
185East Indian ebony1,630 lbf
186Opepe1,630 lbf
187Panga Panga1,630 lbf
188Swamp white oak1,620 lbf
189Carbonero1,615 lbf
190Tauroniro1,610 lbf
191Abiurana-brancaMicropholis mensalis1,605 lbf
192Peroba de campos1,600 lbf
193Kasai1,595 lbf
194Cordyla1,580 lbf
195Honeylocust1,580 lbf
196TauariCouratari stellata1,565 lbf
197Afrormosia1,560 lbf
198Resak1,550 lbf
199Dahoma1,540 lbf
200Timborana1,537 lbf
201Faveira-amargosaVatairea guianensis1,532 lbf
202Breu-preto1,517 lbf
203Camaçari1,515 lbf
204Rose-Mapie1,515 lbf
205Pin oak1,510 lbf
206Sapele1,510 lbf
207Taxi1,505 lbf
208Merbau1,500 lbf
209Grumixava1,490 lbf
210Cherrybark oak1,480 lbf
211Muninga1,480 lbf
212Taxi-pitombaTachigali poeppigiana = Sclerolobium poeppigianum1,479 lbf
213Bintangor1,475 lbf
214Castanheira1,470 lbf
215Sweet birch1,470 lbf
216Embira-pretaGuatteria procera1,468 lbf
217CopaíbaCopaifera duckei1,464 lbf
218CopaíbaCopaifera reticulata1,464 lbf
219NeemAzadirachta spp.1,460 lbf
220Willow oak1,460 lbf
221Pillarwood1,450 lbf
222Sugar maple1,450 lbf
223Long John1,430 lbf
224QuarubaVochysia guianensis1,427 lbf
225Melancieira1,424 lbf
226Angelim1,422 lbf
227Mbarika1,420 lbf
228Ingá / ingá xixi1,418 lbf
229Jagua1,410 lbf
230Sepetir1,410 lbf
231Tawa1,405 lbf
232Sabicú1,400 lbf
233Scarlet oak1,400 lbf
234Enbira-preta1,396 lbf
235Muiratinga1,389 lbf
236Guariúba1,380 lbf
237Taxi-pitombaTachigali chrysophylla =Sclerolobium chrysophyllum1,378 lbf
238TentoOrmosia coccinea1,378 lbf
239White Cypress-Pine1,375 lbf
240Cedro1,373 lbf
241Bishopwood1,370 lbf
242Bur oak1,370 lbf
243Kulim1,370 lbf
244Mafu1,370 lbf
245Berlinia1,360 lbf
246Post oak1,360 lbf
247White oak1,360 lbf
248Putat Paya1,355 lbf
249MandioqueiraRuizterania albiflora = Qualea albiflora1,351 lbf
250Musine1,350 lbf
251Capomo1,340 lbf
252Sorva1,329 lbf
253Tasmanian-Myrtle1,325 lbf
254Rock elm1,320 lbf
255White ash1,320 lbf
256Chickrassy1,310 lbf
257Fava-branca1,310 lbf
258Angelim-pedraHymenolobium petraeum1,301 lbf
259American beech1,300 lbf
260principally G, bancanus1,300 lbf
261Ramin1,300 lbf
262Angelique1,290 lbf
263Mansonia1,290 lbf
264Mersawa1,290 lbf
265Northern red oak1,290 lbf
266IpêTabebuia sp1,280 lbf
267Keruing1,270 lbf
268Itaúba / itaúba-vermelha1,262 lbf
269Iroko1,260 lbf
270Utile1,260 lbf
271Yellow birch1,260 lbf
272Angelim-pedraHymenolobium nitidum1,257 lbf
273LouroAnaueria brasiliensis = Beilschmiedia brasiliensis1,257 lbf
274Molave1,255 lbf
275Thingan1,255 lbf
276Amapá-doceBrosimum parinarioides1,250 lbf
277Bitter Angelim1,250 lbf
278Keledang1,250 lbf
279Simpoh1,250 lbf
280Tchitola1,250 lbf
281Needlewood1,245 lbf
282Caribbean pine1,240 lbf
283Kokko1,240 lbf
284Swamp chestnut oak1,240 lbf
285Ayan1,230 lbf
286Kapur1,230 lbf
287Mengkulang1,230 lbf
288Yellow Sanders1,220 lbf
289Black oak1,210 lbf
290Laurel oak1,210 lbf
291Ararapari1,208 lbf
292Angelim-pedraHymenolobium pulcherrimum1,206 lbf
293Narra1,202 lbf
294Green ash1,200 lbf
295Kelat1,198 lbf
296LouroOcotea sp.1,198 lbf
297UcuubaranaIryanthera grandis1,195 lbf
298Overcup oak1,190 lbf
299Water oak1,190 lbf
300White Chuglam1,190 lbf
301Amapá-doceBrosimum potabile1,184 lbf
302Black maple1,180 lbf
303Okwen1,180 lbf
304QuarubaVochysia obidensis1,179 lbf
305Taxi-preto / ziquita1,166 lbf
306Fiddlewood1,160 lbf
307Oregon ash1,160 lbf
308Arapari1,153 lbf
309Seru1,153 lbf
310Santa Maria1,150 lbf
311Pipli1,145 lbf
312Haldu1,140 lbf
313White meranti1,140 lbf
314TauariCouratari guianensis1,138 lbf
315Louro-mamorim1,135 lbf
316Pequiá1,133 lbf
317Andiroba1,130 lbf
318Chestnut oak1,130 lbf
319Manni1,120 lbf
320MururéBrosimum acutifolium subsp interjectum1,120 lbf
321Yellow Sterculia1,120 lbf
322Embira-branca1,118 lbf
323Thitka1,118 lbf
324Makoré1,110 lbf
325Australian Blackwood1,100 lbf
326Niangon1,100 lbf
327Monjoleiro1,093 lbf
328Magnolia1,090 lbf
329Odoko1,090 lbf
330Avodire1,080 lbf
331Merpauh1,075 lbf
332Garrote1,074 lbf
333MandioqueiraQualea gracilior = Qualea cf lancifolia1,071 lbf
334Xixá1,071 lbf
335White Bombay1,070 lbf
336CopaíbaCopaifera multijuga1,067 lbf
337Cramantee1,065 lbf
338Louro-pretoOcotea fragrantissima1,063 lbf
339Canelo1,060 lbf
340Southern red oak1,060 lbf
341Pyinma1,055 lbf
342Faveira-amargosaVataireopsis speciosa1,043 lbf
343Virola1,041 lbf
344Sumaúma-da-terra-firme1,034 lbf
345Arariba1,030 lbf
346Abacatirana1,025 lbf
347Albarco1,020 lbf
348Darah Darah1,020 lbf
349Southern magnolia1,020 lbf
350Pau-ponga1,019 lbf
351Nyatoh1,018 lbf
352Black walnut1,010 lbf
353Louro-pretoOcotea neesiana1,010 lbf
354CopaíbaCopaifera sp.1,007 lbf
355Baracara1,000 lbf
356Guarea1,000 lbf
357Laurel Blanco1,000 lbf
358MangoMangifera spp.1,000 lbf
359Teak1,000 lbf
360FreijóCordia goeldiana996 lbf
361Aningeria995 lbf
362Itaúba992 lbf
363Rauli990 lbf
364Cow Tree980 lbf
365Paldao980 lbf
366QuarubaVochysia maxima976 lbf
367Tauari-vermelho970 lbf
368FreijóCordia bicolor963 lbf
369Robe960 lbf
370Albizzia955 lbf
371Inga-de-porco955 lbf
372Pterygota955 lbf
373RoxinhoParkia pendula952 lbf
374Black cherry950 lbf
375Imbuia950 lbf
376Red maple950 lbf
377Breu-branco948 lbf
378Angélica946 lbf
379Janitá / garrote946 lbf
380African-Walnut940 lbf
381Gedu Nohor940 lbf
382TauariCouratari oblongifolia936 lbf
383East African Camphorwood930 lbf
384Kirikawa930 lbf
385Ocote pine910 lbf
386Paper birch910 lbf
387Punah910 lbf
388Ekebergia900 lbf
389Estribeiro900 lbf
390Gommier900 lbf
391Sande900 lbf
392Amoora895 lbf
393Tatapiririca891 lbf
394Embira-pretaDiclinanona calycina888 lbf
395Embira-pretaGuatteria olivacea883 lbf
396FreijóCordia sagotii882 lbf
397Cerejeira880 lbf
398Hackberry880 lbf
399Water tupelo880 lbf
400BreuProtium heptaphyllum877 lbf
401Cedrinho874 lbf
402Longleaf pine870 lbf
403Embira864 lbf
404Lingue860 lbf
405Slippery elm860 lbf
406Bigleaf maple850 lbf
407Black ash850 lbf
408Samán850 lbf
409Sweetgum850 lbf
410Idígbo845 lbf
411Silky-Oak840 lbf
412White Seraya838 lbf
413African mahogany830 lbf
414American elm830 lbf
415Podo830 lbf
416Western larch830 lbf
417Taxi-branco818 lbf
418UcuubaranaOsteophloeum platyspermum817 lbf
419Black tupelo810 lbf
420True mahogany800 lbf
421Sterculia798 lbf
422Maminha-de-porca791 lbf
423Amburana790 lbf
424Amapa amargoso789 lbf
425Morototó789 lbf
426Tornillo787 lbf
427Rimú785 lbf
428Abura780 lbf
429Dark red meranti780 lbf
430Parana-pine780 lbf
431American sycamore770 lbf
432Ramón770 lbf
433Yellow meranti770 lbf
434Podocarp760 lbf
435Louro-vermelho756 lbf
436Radiata pine750 lbf
437Faveira / visgueiro743 lbf
438Agba740 lbf
439Mtambara740 lbf
440Virginia pine740 lbf
441Angelica Tree725 lbf
442Champaca725 lbf
443Queensland-Maple725 lbf
444Baromalli720 lbf
445Jongkong720 lbf
446Muirungi720 lbf
447PochoteBombacopsis quinata720 lbf
448Coast Douglas-fir710 lbf
449Ogea710 lbf
450Cauchorana703 lbf
451Cucumbertree700 lbf
452Djedoe700 lbf
453Lechero700 lbf
454Silver maple700 lbf
455Amescla697 lbf
456Tamboril691 lbf
457Haiari690 lbf
458Loblolly pine690 lbf
459Shortleaf pine690 lbf
460White lauan690 lbf
461Axixá686 lbf
462DurianDurio spp.680 lbf
463Mountain hemlock680 lbf
464Vitex680 lbf
465African Canaríum670 lbf
466FaveiraParkia multijuga668 lbf
467Determa660 lbf
468Interior West Douglas-fir660 lbf
469Primavera660 lbf
470Spruce pine660 lbf
471CajuaçuAnacardium parvifolium657 lbf
472Totara655 lbf
473Cativo630 lbf
474Machilus630 lbf
475Port-Orford cedar630 lbf
476Virola / ucuúba-cheirosa624 lbf
477Gmelina622 lbf
478FaveiraParkia nitida = Parkia oppositifolia621 lbf
479Merkus Pine620 lbf
480Ilomba610 lbf
481Benguet Pine605 lbf
482Yemeri605 lbf
483Interior North Douglas-fir600 lbf
484KadamAnthocephalus chinensis600 lbf
485Musizi600 lbf
486Spanish-cedar600 lbf
487CajuaçuAnacardium occidentale = Anacardium microcarpum591 lbf
488Red alder590 lbf
489Tamarack590 lbf
490West African Cordia590 lbf
491Pinho-cuiabano586 lbf
492Castanha-de-arara582 lbf
493Yellow cedar580 lbf
494Jack pine570 lbf
495Medang562 lbf
496Alerce560 lbf
497CajuaçuAnacardium spruceanum560 lbf
498Red pine560 lbf
499Pau-de-jangada558 lbf
500Hura550 lbf
501Toon550 lbf
502American chestnut540 lbf
503Western hemlock540 lbf
504Yellow-poplar540 lbf
505Black spruce530 lbf
506Red spruce530 lbf
507Guanacaste520 lbf
508Baldcypress510 lbf
509Banak510 lbf
510Interior South Douglas-fir510 lbf
511Sitka spruce510 lbf
512CajuaçuAnacardium giganteum505 lbf
513Antíaris500 lbf
514California red fir500 lbf
515Eastern hemlock500 lbf
516Ucuúba / virola496 lbf
517Butternut490 lbf
518Grand fir490 lbf
519Limba490 lbf
520Lodgepole pine480 lbf
521Old-growth redwood480 lbf
522White fir480 lbf
523Deglupta470 lbf
524Espave470 lbf
525Incense cedar470 lbf
526Fava-bolota / visgueiro463 lbf
527Magas462 lbf
528Light red meranti460 lbf
529Mexican cypress460 lbf
530Ponderosa pine460 lbf
531Pulai460 lbf
532Marupá452 lbf
533Urucu-da-mata437 lbf
534Eastern cottonwood430 lbf
535Obeche430 lbf
536Pacific silver fir430 lbf
537Sajo425 lbf
538Caroba / parapará423 lbf
539Western white pine420 lbf
540Young-growth redwood420 lbf
541Alstonia410 lbf
542American basswood410 lbf
543Noble fir410 lbf
544White spruce410 lbf
545Bombax400 lbf
546Chicha400 lbf
547Engelmann spruce390 lbf
548Jelutong390 lbf
549Balsam fir380 lbf
550Cuangare380 lbf
551Eastern white pine380 lbf
552Okoume380 lbf
553Sugar pine380 lbf
554Leiteiro379 lbf
555Binuang362 lbf
556Mastate360 lbf
557Cajá359 lbf
558Atlantic white cedar350 lbf
559Black cottonwood350 lbf
560Quaking aspen350 lbf
561Subalpine fir350 lbf
562Western redcedar350 lbf
563Cananga330 lbf
564Burra-leiteira324 lbf
565Northern white cedar320 lbf
566Trumpet-Wood320 lbf
567Caucho313 lbf
568Figueira / gameleira269 lbf
569Duru250 lbf
570Ceiba240 lbf
571Balsa88 lbf

How to read this chart

A Janka number describes one board of one tree at one moisture content. Two boards of the same species can differ by a fifth. Treat the number as a rank, and not as a specification.

Values here are for wood at 12% moisture content. A green board tests softer.