North America · softwood
Eastern hemlock
Tsuga canadensis, Pinaceae
Read the practical guide to Eastern hemlockJanka hardness
500 lbf
Harder than 10% of the 571 species with a laboratory test.
At a glance
- Janka hardness
- 500 lbf
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Density
- 28.0 lb/ft³
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Volumetric shrinkage
- 9.7%
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
- Availability · editorial
- Widely stocked
Working characteristics: Eastern hemlock splinters easily when worked with tools. Alden — Softwoods of North America (1997), FPL-GTR-102
Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.
Sourced wood and tree images
Each image names its author, its licence, and the page it came from.

WoodFamartin · CC BY-SA 4.0 · Wikimedia Commons 
WoodFamartin · CC BY-SA 4.0 · Wikimedia Commons 
WoodFamartin · CC BY-SA 4.0 · Wikimedia Commons 
BarkPhoto (c)2007 Derek Ramsey (Ram-Man) · CC BY-SA 2.5 · Wikimedia Commons 
BarkPhoto (c)2007 Derek Ramsey (Ram-Man) · CC BY-SA 2.5 · Wikimedia Commons 
TrunkFamartin · CC BY-SA 4.0 · Wikimedia Commons 
TrunkFamartin · CC BY-SA 4.0 · Wikimedia Commons 
TreeBruce Marlin · CC BY-SA 3.0 · Wikidata via Wikimedia Commons 
TreeIan Manning · CC BY · iNaturalist 
TreeDouglas Goldman · CC BY-SA · iNaturalist
Geographic distribution
Where it grows
Recorded distribution of Tsuga canadensis. Native areas are part of its natural range; introduced areas are places where it has been brought by people.
Loading world map…
Native range (28 regions)
Alabama · Connecticut · Georgia · Indiana · Kentucky · Maine · Maryland · Massachusetts · Michigan · Minnesota · New Brunswick · New Hampshire · New Jersey · New York · North Carolina · Nova Scotia · Ohio · Ontario · Pennsylvania · Prince Edward I. · Québec · Rhode I. · South Carolina · Tennessee · Vermont · Virginia · West Virginia · Wisconsin
Introduced range (4 regions)
Germany · Great Britain · Norway · Poland
Shading marks botanical regions with recorded presence, not the exact extent of forests or commercial plantations. Large countries may be divided into states or provinces. Extinct and doubtful records are excluded. Unshaded areas have no record in this dataset; they do not prove absence.
Source: Kew species record · WCVP, version 16 (June 2026), Royal Botanic Gardens, Kew, CC BY 3.0. Map boundaries: TDWG / WGSRPD; adapted to a world map.
Measured properties
Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.
- Janka hardness
- 500 lbf
- Density at 12% MC
- 28.0 lb/ft³
- Specific gravity
- 0.40
- Modulus of rupture
- 8,900 lb/in²
- Modulus of elasticity
- 1.20 ×10⁶ lb/in²
- Crushing strength
- 5,410 lb/in²
- Radial shrinkage
- 3.0%
- Tangential shrinkage
- 6.8%
- Volumetric shrinkage
- 9.7%
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Where these numbers come from
Check the references below to see which properties each source supports.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Janka hardness · Green wood hardness · Specific gravity · Basic specific gravity · Density · Bending strength · Stiffness · Crushing strength · Green wood properties
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Shrinkage
- USDA FIA REF_SPECIES
Scientific name
- GWDD v2.2 (Fischer et al. 2026)
Botanical family
Eastern hemlock wood: a practical guide
Eastern hemlock (Tsuga canadensis) is listed as a softwood from North America. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.
Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.
What is Eastern hemlock?
The botanical name used by this record is Tsuga canadensis, in the Pinaceae family. When buying, ask the supplier to identify the species rather than relying on the common name alone.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga canadensis
Eastern hemlock is native to Cape Breton Islands, Nova Scotia, Prince Edward Island, New Brunswick, the Gaspe’ Peninsula of southern Quebec and Maine, west to southern Ontario, northern Michigan, Wisconsin, and eastern Minnesota, south to Indiana and east to Ohio, Pennsylvania, Maryland and New Jersey and south in the mountains to northwestern South Carolina, northern Georgia and northern Alabama. The production of eastern hemlock lumber is divided fairly evenly between the New England States, the Middle Atlantic States, and the Lake States.
Common names can vary between countries and suppliers. For a restoration, repeat order, or technical specification, keep the botanical name and the supplier’s description with the material record.
A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.
General workshop reference: USDA Wood Handbook (public domain)
Color, grain, and choosing visible boards
The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga canadensis
The heartwood of eastern hemlock is pale brown with a reddish hue. The sapwood is not distinctly separated from the heartwood but may be lighter in color. The wood is coarse and uneven in texture (old trees tend to have considerable shake); it is moderately light in weight, moderately hard, moderately low in strength, moderately limber, and moderately low in shock resistance.
For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.
- Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
- Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
- Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.
General workshop reference: USDA Wood Handbook (public domain)
Hardness, weight, and strength in practice
Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.
- Janka hardness: 500 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Density: 28.0 lb/ft³.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Bending strength: 8,900 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Stiffness: 1.20 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Compression parallel to grain: 5,410 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
Uses and project selection for Eastern hemlock
The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga canadensis
Eastern hemlock is used principally for lumber and pulpwood. The lumber is used in building construction for framing, sheathing, subflooring, and roof boards, and in the manufacture of boxes, pallets, and crates.
Allow for visible dents on a heavily used surface. This hardness may be workable for many interior parts, but a tabletop or floor also needs a suitable finish and a realistic maintenance plan.
Based on the recorded density, handling weight may be an advantage for larger parts. Check the actual stock and design connections for its properties rather than substituting dimensions from a heavier wood.
- Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
- Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
- Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
- Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.
General workshop reference: USDA Wood Handbook (public domain)
Sawing, planing, routing, and drilling
Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga canadensis
Eastern hemlock splinters easily when worked with tools. It is low in splitting resistance and average in nail-holding capacity. It glues easily and is moderate in paint-holding ability.
- Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
- Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
- Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
- Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
- Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
- Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.
General workshop reference: USDA Wood Handbook (public domain)
Drying, shrinkage, and seasonal movement
Recorded green-to-ovendry shrinkage: radial 3.0%; tangential 6.8%; volumetric 9.7%. Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3 (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.
Tangential shrinkage is about 2.3 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.
Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.
- Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
- Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
- Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.
General workshop reference: USDA Wood Handbook (public domain)
Gluing and assembly
Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.
A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.
Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.
General workshop reference: USDA Wood Handbook (public domain)
Finishing, staining, and surface preparation
Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.
Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.
- Prepare consistently: remove marks from each sanding stage and inspect under raking light.
- Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
- Include end grain: test it when it will remain visible, since it can take color differently from the face.
- Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.
General workshop reference: USDA Wood Handbook (public domain)
Decay resistance, exposure, and care
Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga canadensis
The heartwood of eastern hemlock is slightly resistant to nonresistant to decay.
For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.
For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.
General workshop reference: USDA Wood Handbook (public domain)
Buying Eastern hemlock: a practical checklist
Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.
For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.
- Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
- Moisture: ask about drying history and check the stock against the intended application.
- Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
- Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
- Specification: obtain appropriate grade or product evidence for structural or demanding service.
- Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.
General workshop reference: USDA Wood Handbook (public domain)
Dust, food contact, and care
The dedicated occupational-source dataset has no reaction report linked to this entry. Historical descriptions may discuss additional handling concerns. An absent report does not establish that dust is harmless or that the wood is suitable for food contact. Use appropriate dust control and follow the controls for the tools and materials you use.
For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.
- Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
- Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
- Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.
Comparing alternatives
The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.
| Wood | Janka | Density |
|---|---|---|
| Eastern hemlockTsuga canadensis | 500 lbf | 28.0 lb/ft³ |
| Western hemlockTsuga heterophylla | 540 lbf | 31.5 lb/ft³ |
| Mountain hemlockTsuga mertensiana | 680 lbf | 31.5 lb/ft³ |
| BaldcypressTaxodium distichum | 510 lbf | 32.2 lb/ft³ |
Before you build
- Confirm the species and the usable dimensions of the stock.
- Check the properties that matter to the part, including any estimates or gaps.
- Match moisture to the intended environment and allow cross-grain movement.
- Make representative cutting, bonding, and finishing trials.
- Keep the approved sample, product details, and care instructions with the job.
Sources and further reading
Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.
- Alden — Softwoods of North America (1997), FPL-GTR-102
Tsuga canadensis · species description · public domain. Historical species descriptions. Nursery, medicinal, and industrial uses mentioned by the source are not instructions for making a product.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
public domain. Supports: janka lbf, janka n, janka green lbf, specific gravity 12, specific gravity basic, density kg m3, mor psi, moe mpsi, crushing psi, green.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
public domain. Supports: shrinkage.
- USDA FIA REF_SPECIES
public domain. Supports: scientific name.
- GWDD v2.2 (Fischer et al. 2026)
CC BY 4.0. Supports: family.
- USDA FPL — Wood Handbook (2021)
Public domain. Chapters on moisture, mechanical properties, fastenings, design, bonding, drying, decay, preservation, and finishing provide the general workshop background.
- USDA FSIS — Cutting Boards
Public domain. Cleaning, cross-contamination prevention, and board replacement.
Compare before you choose
See how Eastern hemlock and Western hemlock differ in hardness, density, strength, and shrinkage, with sources alongside the values.
Compare Eastern hemlock with Western hemlockWoods of similar hardness
A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.
| # | Wood | Janka | |
|---|---|---|---|
| 1 | Antíaris | 500 lbf | |
| 2 | California red fir | 500 lbf | |
| 3 | Ucuúba / virola | 496 lbf | |
| 4 | CajuaçuAnacardium giganteum | 505 lbf | |
| 5 | Black poplar | 509 lbf* | |
| 6 | Chinese catalpa | 509 lbf* |