North America · softwood
Western hemlock
Tsuga heterophylla, Pinaceae
Read the practical guide to Western hemlockJanka hardness
540 lbf
Harder than 12% of the 571 species with a laboratory test.
At a glance
- Janka hardness
- 540 lbf
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Density
- 31.5 lb/ft³
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Volumetric shrinkage
- 12.4%
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
- Availability · editorial
- Widely stocked
Working characteristics: The wood is intermediate in nail-holding ability and has a tendency to split when nailed. Alden — Softwoods of North America (1997), FPL-GTR-102
Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.
Sourced wood and tree images
Each image names its author, its licence, and the page it came from.

TreeDoug Kerr from Albany, NY, United States · CC BY-SA 2.0 · Wikidata via Wikimedia Commons 
TreeLyrae · CC BY · iNaturalist
Geographic distribution
Where it grows
Recorded distribution of Tsuga heterophylla. Native areas are part of its natural range; introduced areas are places where it has been brought by people.
Loading world map…
Native range (8 regions)
Alaska · Alberta · British Columbia · California · Idaho · Montana · Oregon · Washington
Introduced range (7 regions)
Denmark · Føroyar · France · Germany · Great Britain · Ireland · Norway
Shading marks botanical regions with recorded presence, not the exact extent of forests or commercial plantations. Large countries may be divided into states or provinces. Extinct and doubtful records are excluded. Unshaded areas have no record in this dataset; they do not prove absence.
Source: Kew species record · WCVP, version 16 (June 2026), Royal Botanic Gardens, Kew, CC BY 3.0. Map boundaries: TDWG / WGSRPD; adapted to a world map.
Measured properties
Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.
- Janka hardness
- 540 lbf
- Density at 12% MC
- 31.5 lb/ft³
- Specific gravity
- 0.45
- Modulus of rupture
- 11,300 lb/in²
- Modulus of elasticity
- 1.63 ×10⁶ lb/in²
- Crushing strength
- 7,200 lb/in²
- Radial shrinkage
- 4.2%
- Tangential shrinkage
- 7.8%
- Volumetric shrinkage
- 12.4%
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Where these numbers come from
Check the references below to see which properties each source supports.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Janka hardness · Green wood hardness · Specific gravity · Basic specific gravity · Density · Bending strength · Stiffness · Crushing strength · Green wood properties
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Shrinkage
- USDA FIA REF_SPECIES
Scientific name
- GWDD v2.2 (Fischer et al. 2026)
Botanical family
Western hemlock wood: a practical guide
Western hemlock (Tsuga heterophylla) is listed as a softwood from North America. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.
Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.
What is Western hemlock?
The botanical name used by this record is Tsuga heterophylla, in the Pinaceae family. When buying, ask the supplier to identify the species rather than relying on the common name alone.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga heterophylla
Western hemlock is native to the Pacific Coast region from southern Alaska (Kenai Peninsula) southeast through southeastern Alaska and western British Columbia to western Washington, western Oregon, and northwestern California. It is also found in the Rocky Mountain region from southeastern British Columbia south to northeastern Washington, northern Idaho, and northwestern Montana.
Common names can vary between countries and suppliers. For a restoration, repeat order, or technical specification, keep the botanical name and the supplier’s description with the material record.
A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.
General workshop reference: USDA Wood Handbook (public domain)
Color, grain, and choosing visible boards
The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga heterophylla
The heartwood and sapwood of western hemlock are almost white with a purplish tinge. The sapwood, which is sometimes lighter in color, is generally not more than 1 in. (2.54 cm) thick. The wood often contains small, sound, black knots that are usually tight and stay in place. Dark streaks are often found in the lumber; these are caused by hemlock bark maggots and generally do not reduce strength. Western hemlock is moderately light in weight and moderate in strength. It is moderate in its hardness, stiffness, and shock resistance. It has moderately high shrinkage, about the same as Douglas-fir. Green hemlock lumber contains considerably more water than Douglas-fir, and requires longer kiln drying time. Trees may contain wetwood and/or have ring shake.
For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.
- Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
- Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
- Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.
General workshop reference: USDA Wood Handbook (public domain)
Hardness, weight, and strength in practice
Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.
- Janka hardness: 540 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Density: 31.5 lb/ft³.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Bending strength: 11,300 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Stiffness: 1.63 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Compression parallel to grain: 7,200 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
Uses and project selection for Western hemlock
The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga heterophylla
Western hemlock is used for pulpwood, lumber, roof decking, laminating stock, mouldings, architectural trim, general construction, newsprint, and plywood. The lumber is used extensively for building material, such as sheathing, siding, subflooring, joists, studding, planking, and rafters. Considerable quantities are used in the manufacture of boxes, pallets, crates, and flooring, and smaller amounts for furniture and ladders.
Allow for visible dents on a heavily used surface. This hardness may be workable for many interior parts, but a tabletop or floor also needs a suitable finish and a realistic maintenance plan.
Based on the recorded density, calculate the weight of the finished volume before choosing hardware or building a portable piece. Moisture content and individual boards can change the result.
- Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
- Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
- Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
- Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.
General workshop reference: USDA Wood Handbook (public domain)
Sawing, planing, routing, and drilling
Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga heterophylla
The wood is intermediate in nail-holding ability and has a tendency to split when nailed. It glues, stains, polishs, varnishs, and paints satisfactorily.
- Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
- Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
- Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
- Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
- Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
- Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.
General workshop reference: USDA Wood Handbook (public domain)
Drying, shrinkage, and seasonal movement
Recorded green-to-ovendry shrinkage: radial 4.2%; tangential 7.8%; volumetric 12.4%. Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3 (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.
Tangential shrinkage is about 1.9 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.
Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.
- Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
- Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
- Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.
General workshop reference: USDA Wood Handbook (public domain)
Gluing and assembly
Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.
A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.
Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.
General workshop reference: USDA Wood Handbook (public domain)
Finishing, staining, and surface preparation
Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.
Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.
- Prepare consistently: remove marks from each sanding stage and inspect under raking light.
- Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
- Include end grain: test it when it will remain visible, since it can take color differently from the face.
- Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.
General workshop reference: USDA Wood Handbook (public domain)
Decay resistance, exposure, and care
Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Tsuga heterophylla
The heartwood of hemlock is slightly resistant to nonresistant to decay.
For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.
For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.
General workshop reference: USDA Wood Handbook (public domain)
Buying Western hemlock: a practical checklist
Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.
For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.
- Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
- Moisture: ask about drying history and check the stock against the intended application.
- Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
- Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
- Specification: obtain appropriate grade or product evidence for structural or demanding service.
- Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.
General workshop reference: USDA Wood Handbook (public domain)
Dust, food contact, and care
The occupational-source record linked to Western hemlock reports bronchial effects, rhinitis. The botanical name matched the source entry, so this record is about this species.
Read the reported effects, source evidence, and match confidence for Western hemlock.
For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.
- Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
- Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
- Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.
Comparing alternatives
The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.
| Wood | Janka | Density |
|---|---|---|
| Western hemlockTsuga heterophylla | 540 lbf | 31.5 lb/ft³ |
| Eastern hemlockTsuga canadensis | 500 lbf | 28.0 lb/ft³ |
| Mountain hemlockTsuga mertensiana | 680 lbf | 31.5 lb/ft³ |
| Black sprucePicea mariana | 530 lbf | 29.3 lb/ft³ |
Before you build
- Confirm the species and the usable dimensions of the stock.
- Check the properties that matter to the part, including any estimates or gaps.
- Match moisture to the intended environment and allow cross-grain movement.
- Make representative cutting, bonding, and finishing trials.
- Keep the approved sample, product details, and care instructions with the job.
Sources and further reading
Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.
- Alden — Softwoods of North America (1997), FPL-GTR-102
Tsuga heterophylla · species description · public domain. Historical species descriptions. Nursery, medicinal, and industrial uses mentioned by the source are not instructions for making a product.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
public domain. Supports: janka lbf, janka n, janka green lbf, specific gravity 12, specific gravity basic, density kg m3, mor psi, moe mpsi, crushing psi, green.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
public domain. Supports: shrinkage.
- USDA FIA REF_SPECIES
public domain. Supports: scientific name.
- GWDD v2.2 (Fischer et al. 2026)
CC BY 4.0. Supports: family.
- USDA FPL — Wood Handbook (2021)
Public domain. Chapters on moisture, mechanical properties, fastenings, design, bonding, drying, decay, preservation, and finishing provide the general workshop background.
- USDA FSIS — Cutting Boards
Public domain. Cleaning, cross-contamination prevention, and board replacement.
Compare before you choose
See how Western hemlock and Eastern hemlock differ in hardness, density, strength, and shrinkage, with sources alongside the values.
Compare Western hemlock with Eastern hemlockHealth and safety
A published occupational source reports bronchial effects, rhinitis for this wood. What that means, and how strong the link is.
Woods of similar hardness
A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.
| # | Wood | Janka | |
|---|---|---|---|
| 1 | American chestnut | 540 lbf | |
| 2 | Yellow-poplar | 540 lbf | |
| 3 | Adoung | 542 lbf* | |
| 4 | Chinese tallow | 542 lbf* | |
| 5 | Cigarbush | 542 lbf* | |
| 6 | Hinchahuevos | 542 lbf* |