Africa · hardwood
Iroko
Chlorophora spp., Moraceae
Also sold as: Semli, Odoum, Rokko, Oroko, Abang, Mandji, Mereira, Kambala, Mvule
Read the practical guide to IrokoJanka hardness
1,260 lbf
Harder than 53% of the 571 species with a laboratory test.
At a glance
- Janka hardness
- 1,260 lbf
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
- Density
- 43.0 lb/ft³
- Chudnoff 1984, Tropical Timbers of the World (AH-607)
- Volumetric shrinkage
- 8.8%
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
- Availability · editorial
- Widely stocked
Working characteristics need separate confirmation; this record has no species-specific published description.
Missing evidence: species-specific working description, species-specific durability description.
Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.
Sourced wood and tree images
No species-specific open-licence image was found in our current sources. These show other species of Chlorophora. A sample of the genus is a guide to colour and grain, not a record of this wood.

Woodgenus, not this speciesCirad · Public domain · Cirad xylothèque via Wikimedia Commons 
Woodgenus, not this speciesCirad · Public domain · Cirad xylothèque via Wikimedia Commons 
Woodgenus, not this speciesCirad · Public domain · Cirad xylothèque via Wikimedia Commons
Geographic distribution
Where it grows
A reliable species-level range is not yet available for this record. Some wood names cover several species, and some scientific names need further verification. We’ll add a map when the name can be matched to a documented distribution.
Measured properties
Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.
- Janka hardness
- 1,260 lbf
- Density at 12% MC
- 43.0 lb/ft³
- Specific gravityestimate
- 0.59
- Modulus of rupture
- 12,400 lb/in²
- Modulus of elasticity
- 1.46 ×10⁶ lb/in²
- Crushing strength
- 7,590 lb/in²
- Radial shrinkage
- 2.8%
- Tangential shrinkage
- 3.8%
- Volumetric shrinkage
- 8.8%
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Chudnoff 1984, Tropical Timbers of the World (AH-607)
USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Where these numbers come from
Check the references below to see which properties each source supports.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Janka hardness · Green wood hardness · Basic specific gravity · Bending strength · Stiffness · Crushing strength · Green wood properties
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Shrinkage
- Chudnoff 1984, Tropical Timbers of the World (AH-607)
Botanical family · Density
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Specific gravity
One value on this page is an estimate. Estimates use the specific-gravity conversions or regressions identified in the source records. An estimate is not a test result. Each one carries a mark.
Iroko wood: a practical guide
Iroko (Chlorophora spp.) is listed as a hardwood from Africa. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.
Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.
What is Iroko?
The botanical name used by this record is Chlorophora spp., in the Moraceae family. Other names recorded here include Semli, Odoum, Rokko, Oroko, Abang, Mandji, Mereira, Kambala, Mvule.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora tinctoria. This passage describes this identified member, not every species sold under the page’s group name.
Widely distributed throughout tropical America. A northern form is found in coastal lowlands of southern Mexico, Central America, the West Indies, and northern South America. A southern form is found in Misiones (Argentina), Paraguay, and southern Brazil, but nowhere abundant.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora excelsa. This passage describes this identified member, not every species sold under the page’s group name.
The two species, between them, extend across the entire width of tropical Africa. C. regia limited to the extreme west of Africa from Gambia to Ghana and is less drought resistant.
The botanical label represents a group rather than a single identified species. Material sold under it may include different species, and a property reported for that group is not a guarantee for every board.
A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.
General workshop reference: USDA Wood Handbook (public domain)
Color, grain, and choosing visible boards
The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora tinctoria. This passage describes this identified member, not every species sold under the page’s group name.
Fresh heartwood is bright yellow, drying to golden yellow, changing upon exposure to brown or russet, sometimes with a reddish tinge; sharply demarcated from the nearly white sapwood. Luster high; texture usually fine; grain variable, often interlocked; odor and taste lacking or not distinctive.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora excelsa. This passage describes this identified member, not every species sold under the page’s group name.
Heartwood varies from a pale yellowish brown to dark chocolate brown with lighter markings most conspicuous on flat-sawn surfaces; sapwood yellowish white, clearly demarcated. Texture medium to coarse; grain typically interlocked, sometimes irregular; slightly greasy feel; without odor; wet sawdust may cause dermatitis; occasional large "stone" deposits of calcium carbonate.
For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.
- Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
- Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
- Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.
General workshop reference: USDA Wood Handbook (public domain)
Hardness, weight, and strength in practice
Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.
- Janka hardness: 1,260 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
- Density: 43.0 lb/ft³.Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).
- Bending strength: 12,400 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
- Stiffness: 1.46 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
- Compression parallel to grain: 7,590 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
Uses and project selection for Iroko
The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora tinctoria. This passage describes this identified member, not every species sold under the page’s group name.
Heavy construction, decking, planking, and framing for boats, exterior and interior flooring, turnery, furniture parts, tool handles, railroad ties, and wood tanks. Also contains the coloring maclurin long used as a yellowish-brown or khaki dye.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora excelsa. This passage describes this identified member, not every species sold under the page’s group name.
Suggested as a teak substitute. Joinery, boatbuilding, piling and marine work, domestic flooring, furniture, veneer, railroad crossties, cabinetwork, shop fittings.
Dent resistance is worth considering for furniture and working surfaces. Sharp tools, sound joints, and adequate thickness still determine whether the finished part works well.
Based on the recorded density, calculate the weight of the finished volume before choosing hardware or building a portable piece. Moisture content and individual boards can change the result.
- Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
- Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
- Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
- Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.
General workshop reference: USDA Wood Handbook (public domain)
Sawing, planing, routing, and drilling
Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora excelsa. This passage describes this identified member, not every species sold under the page’s group name.
Works fairly easily with hand or machine tools but with some tearing of interlocked grain; occasional deposits of calcium carbonate severely damage cutting edges; good nailing and gluing characteristics; moderate steam-bending properties; may cause dermatitis in working wet wood.
- Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
- Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
- Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
- Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
- Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
- Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.
General workshop reference: USDA Wood Handbook (public domain)
Drying, shrinkage, and seasonal movement
Recorded green-to-ovendry shrinkage: radial 2.8%; tangential 3.8%; volumetric 8.8%. Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.
Tangential shrinkage is about 1.4 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.
Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.
- Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
- Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
- Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.
General workshop reference: USDA Wood Handbook (public domain)
Gluing and assembly
Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.
A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.
Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.
General workshop reference: USDA Wood Handbook (public domain)
Finishing, staining, and surface preparation
Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.
Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.
- Prepare consistently: remove marks from each sanding stage and inspect under raking light.
- Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
- Include end grain: test it when it will remain visible, since it can take color differently from the face.
- Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.
General workshop reference: USDA Wood Handbook (public domain)
Decay resistance, exposure, and care
Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora tinctoria. This passage describes this identified member, not every species sold under the page’s group name.
Heartwood very durable in resistance to both white-rot and brown-rot fungi and also has excellent weathering characteristics. The heartwood is also rated as highly resistant to dry-wood termites. Data on resistance to marine-borer attack are conflicting.
Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain
Member species: Chlorophora excelsa. This passage describes this identified member, not every species sold under the page’s group name.
Heartwood is very durable and is resistant to termite and marine borer attack as well. Sapwood liable to powder-post beetle attack.
For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.
For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.
General workshop reference: USDA Wood Handbook (public domain)
Buying Iroko: a practical checklist
Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.
For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.
- Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
- Moisture: ask about drying history and check the stock against the intended application.
- Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
- Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
- Specification: obtain appropriate grade or product evidence for structural or demanding service.
- Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.
General workshop reference: USDA Wood Handbook (public domain)
Dust, food contact, and care
The occupational-source record linked to Iroko reports asthma, dermatitis, nettle rash. A source entry for the genus matched. The report belongs to the genus, and this species may differ from its relatives.
Read the reported effects, source evidence, and match confidence for Iroko.
For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.
- Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
- Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
- Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.
Comparing alternatives
The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.
| Wood | Janka | Density |
|---|---|---|
| IrokoChlorophora spp. | 1,260 lbf | 43.0 lb/ft³ |
| SapeleEntandrophragma cylindricum | 1,510 lbf | 42.0 lb/ft³ |
| Panga PangaMillettia spp. | 1,630 lbf | 55.0 lb/ft³ |
| African mahoganyKhaya spp. | 830 lbf | 32.0 lb/ft³ |
Before you build
- Confirm the species and the usable dimensions of the stock.
- Check the properties that matter to the part, including any estimates or gaps.
- Match moisture to the intended environment and allow cross-grain movement.
- Make representative cutting, bonding, and finishing trials.
- Keep the approved sample, product details, and care instructions with the job.
Sources and further reading
Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.
- Chudnoff — Tropical Timbers of the World (1984), AH-607
Chlorophora tinctoria · species description · public domain. Historical descriptions compiled from published literature; uses and durability reports describe the material studied, not a current product approval.
- Chudnoff — Tropical Timbers of the World (1984), AH-607
Chlorophora excelsa · species description · public domain. Historical descriptions compiled from published literature; uses and durability reports describe the material studied, not a current product approval.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
public domain. Supports: janka lbf, janka n, janka green lbf, specific gravity basic, mor psi, moe mpsi, crushing psi, green.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
public domain. Supports: shrinkage.
- Chudnoff 1984, Tropical Timbers of the World (AH-607)
public domain. Supports: family, density kg m3.
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
public domain. Supports: specific gravity 12.
- USDA FPL — Wood Handbook (2021)
Public domain. Chapters on moisture, mechanical properties, fastenings, design, bonding, drying, decay, preservation, and finishing provide the general workshop background.
- USDA FSIS — Cutting Boards
Public domain. Cleaning, cross-contamination prevention, and board replacement.
Compare before you choose
See how Iroko and Sapele differ in hardness, density, strength, and shrinkage, with sources alongside the values.
Compare Iroko with SapeleHealth and safety
A published occupational source reports asthma, dermatitis, nettle rash for this wood. What that means, and how strong the link is.
Woods of similar hardness
A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.
| # | Wood | Janka | |
|---|---|---|---|
| 1 | Utile | 1,260 lbf | |
| 2 | Yellow birch | 1,260 lbf | |
| 3 | Itaúba / itaúba-vermelha | 1,262 lbf | |
| 4 | Angelim-pedraHymenolobium nitidum | 1,257 lbf | |
| 5 | LouroAnaueria brasiliensis = Beilschmiedia brasiliensis | 1,257 lbf | |
| 6 | Alexandrian laurel | 1,255 lbf* |