Wood Record

Oceania · hardwood

Brush Box

Tristania spp., Myrtaceae

Also sold as: Pelawan Pelawan, Keruntum, Pelawan, Selunsur, Melaban, Malabayabas

Read the practical guide to Brush Box

Janka hardness

3,088 lbf

Harder than 94% of the 571 species with a laboratory test.

At a glance

Janka hardness
3,088 lbf
Chudnoff 1984, Tropical Timbers of the World (AH-607)
Density
62.0 lb/ft³
Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage
No published value
Chudnoff 1984, Tropical Timbers of the World (AH-607)
Availability · editorial
Rarely traded

Working characteristics need separate confirmation; this record has no species-specific published description.

Missing evidence: shrinkage, species-specific working description, species-specific durability description.

Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.

Geographic distribution

Where it grows

A reliable species-level range is not yet available for this record. Some wood names cover several species, and some scientific names need further verification. We’ll add a map when the name can be matched to a documented distribution.

Measured properties

Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.

Janka hardness
3,088 lbf

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Density at 12% MC
62.0 lb/ft³

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Specific gravityestimate
0.92

USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

Modulus of rupture
26,200 lb/in²

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Modulus of elasticity
2.68 ×10⁶ lb/in²

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Crushing strength
11,700 lb/in²

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Radial shrinkage
5.0%

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Tangential shrinkage
9.5%

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Volumetric shrinkage
No published test

Chudnoff 1984, Tropical Timbers of the World (AH-607)

Where these numbers come from

Check the references below to see which properties each source supports.

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)

    Botanical family · Janka hardness · Green wood hardness · Basic specific gravity · Density · Bending strength · Stiffness · Crushing strength · Shrinkage

  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

    Specific gravity

One value on this page is an estimate. Estimates use the specific-gravity conversions or regressions identified in the source records. An estimate is not a test result. Each one carries a mark.

Brush Box wood: a practical guide

Brush Box (Tristania spp.) is listed as a hardwood from Oceania. The available descriptive evidence concerns a broader group; the scope is identified beside each source passage. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.

Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.

What is Brush Box?

The botanical name used by this record is Tristania spp., in the Myrtaceae family. Other names recorded here include Pelawan Pelawan, Keruntum, Pelawan, Selunsur, Melaban, Malabayabas.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Tristania spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Indo-Malayan region and extending into Australia, the Philippines, and Indonesia. Some species introduced to other tropical areas.

The botanical label represents a group rather than a single identified species. Material sold under it may include different species, and a property reported for that group is not a guarantee for every board.

A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.

General workshop reference: USDA Wood Handbook (public domain)

Color, grain, and choosing visible boards

The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Tristania spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood pink brown, gray brown, red brown, or dark red; sapwood pink or red brown, lighter than the heartwood, but not always sharply demarcated. Texture medium to fine; grain interlocked, sometimes wavy; somewhat lustrous; without characteristic odor or taste.

For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.

  • Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
  • Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
  • Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.

General workshop reference: USDA Wood Handbook (public domain)

Hardness, weight, and strength in practice

Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.

  • Janka hardness: 3,088 lbf.Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).
  • Density: 62.0 lb/ft³.Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).
  • Bending strength: 26,200 lb/in².Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).
  • Stiffness: 2.68 ×10⁶ lb/in².Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).
  • Compression parallel to grain: 11,700 lb/in².Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain).

Property sources and licences

Uses and project selection for Brush Box

The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Tristania spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Flooring, pallets, heavy construction, specialty items (pulleys, rollers, bearings, sheaves, tool handles).

Surface hardness is a reason to compare this wood for wear, while allowing for greater cutting effort. Make trial cuts and pilot holes before machining or fastening the finished parts.

Based on the recorded density, weight deserves early attention for a large top, door, or portable object. Include the base, hardware, and lifting requirements in the design.

  • Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
  • Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
  • Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
  • Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.

General workshop reference: USDA Wood Handbook (public domain)

Sawing, planing, routing, and drilling

Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Tristania spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Generally difficult to saw and machine because of high density, cutters may dull rapidly (silica content 0.04 to 0.22% but values as high as 3.4% are reported); dresses to a smooth surface; turns excellently.
  • Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
  • Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
  • Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
  • Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
  • Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
  • Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.

General workshop reference: USDA Wood Handbook (public domain)

Drying, shrinkage, and seasonal movement

Recorded green-to-ovendry shrinkage: radial 5.0%; tangential 9.5%; volumetric not reported. Source: Chudnoff 1984, Tropical Timbers of the World (AH-607) (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.

Tangential shrinkage is about 1.9 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.

Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.

  • Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
  • Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
  • Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.

General workshop reference: USDA Wood Handbook (public domain)

Gluing and assembly

Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.

A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.

Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.

General workshop reference: USDA Wood Handbook (public domain)

Finishing, staining, and surface preparation

Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.

Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.

  • Prepare consistently: remove marks from each sanding stage and inspect under raking light.
  • Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
  • Include end grain: test it when it will remain visible, since it can take color differently from the face.
  • Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.

General workshop reference: USDA Wood Handbook (public domain)

Decay resistance, exposure, and care

Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Tristania spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood generally reported to be resistant to attack by decay fungi and termites.

For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.

For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.

General workshop reference: USDA Wood Handbook (public domain)

Buying Brush Box: a practical checklist

Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.

For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.

  • Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
  • Moisture: ask about drying history and check the stock against the intended application.
  • Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
  • Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
  • Specification: obtain appropriate grade or product evidence for structural or demanding service.
  • Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.

General workshop reference: USDA Wood Handbook (public domain)

Dust, food contact, and care

The dedicated occupational-source dataset has no reaction report linked to this entry. Historical descriptions may discuss additional handling concerns. An absent report does not establish that dust is harmless or that the wood is suitable for food contact. Use appropriate dust control and follow the controls for the tools and materials you use.

For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.

  • Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
  • Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
  • Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.

USDA FSIS: Cutting Boards (public domain) · HSE: Wood dust

Comparing alternatives

The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.

Comparison choices are editorial, prioritizing related and commonly traded woods with measured hardness. Estimates are labelled; a dash means no recorded value. Each species links to its full sources.
WoodJankaDensity
Brush BoxTristania spp.3,088 lbf62.0 lb/ft³
Indian rosewoodDalbergia latifolia3,170 lbf53.0 lb/ft³
CumaruDipteryx odorata3,415 lbf66.8 lb/ft³
BubingaGuibourtia spp.2,690 lbf55.9 lb/ft³Estimate

Before you build

  1. Confirm the species and the usable dimensions of the stock.
  2. Check the properties that matter to the part, including any estimates or gaps.
  3. Match moisture to the intended environment and allow cross-grain movement.
  4. Make representative cutting, bonding, and finishing trials.
  5. Keep the approved sample, product details, and care instructions with the job.

Sources and further reading

Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.

Compare before you choose

See how Brush Box and Indian rosewood differ in hardness, density, strength, and shrinkage, with sources alongside the values.

Compare Brush Box with Indian rosewood

Woods of similar hardness

A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.

#WoodJanka
1Honduras Rosewood3,097 lbf*
2IpêHandroanthus serratifolius = Tabebuia serratifolia3,100 lbf
3Sapucaia3,100 lbf
4Cabreúva-parda3,075 lbf
5IngáInga paraensis3,064 lbf
6Australian tallowwood3,054 lbf*

All species