North America · softwood
Interior South Douglas-fir
Pseudotsuga menziesii, Pinaceae
Read the practical guide to Interior South Douglas-firJanka hardness
510 lbf
Harder than 11% of the 571 species with a laboratory test.
At a glance
- Janka hardness
- 510 lbf
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Density
- 32.2 lb/ft³
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
- Volumetric shrinkage
- No published value
- Availability · editorial
- Rarely traded
Working characteristics: Douglas-fir wood is strong, moderately hard, and very stiff. Alden — Softwoods of North America (1997), FPL-GTR-102
Missing evidence: shrinkage.
Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.
Sourced wood and tree images
Each image names its author, its licence, and the page it came from.

WoodCirad · Public domain · Cirad xylothèque via Wikimedia Commons 
WoodCirad · Public domain · Cirad xylothèque via Wikimedia Commons 
WoodNo machine-readable author provided. Lumbar~commonswiki assumed (based on copyri · Public domain · Wikimedia Commons 
WoodCrusier · CC BY 3.0 · Wikimedia Commons 
WoodJean-Pierre Chéreau & Roger Culos · CC BY-SA 3.0 · Wikimedia Commons 
WoodOwn work by the original uploader · Public domain · Wikimedia Commons 
BarkNo machine-readable author provided. Wsiegmund assumed (based on copyright claim · CC BY 2.5 · Wikimedia Commons 
BarkYog Sot · CC0 · Wikimedia Commons 
TreeWalter Siegmund (talk) · CC BY-SA 3.0 · Wikidata via Wikimedia Commons 
TreeDanny Steaven · CC BY-SA · iNaturalist 
TreeEllyne Geurts · CC0 · iNaturalist 
TreeRandal · CC0 · iNaturalist
Geographic distribution
Where it grows
Recorded distribution of Pseudotsuga menziesii. Native areas are part of its natural range; introduced areas are places where it has been brought by people.
Loading world map…
Native range (19 regions)
Alaska · Alberta · Arizona · British Columbia · California · Colorado · Idaho · Mexico Central · Mexico Northeast · Mexico Northwest · Mexico Southwest · Montana · Nevada · New Mexico · Oregon · Texas · Utah · Washington · Wyoming
Introduced range (26 regions)
Austria · Baltic States · Belgium · Bulgaria · Czechoslovakia · Denmark · Finland · Føroyar · France · Germany · Great Britain · Greece · Hungary · Ireland · Italy · New York · Norway · Poland · Portugal · Romania · Spain · Sweden · Switzerland · Tunisia · Turkey · Yugoslavia
Shading marks botanical regions with recorded presence, not the exact extent of forests or commercial plantations. Large countries may be divided into states or provinces. Extinct and doubtful records are excluded. Unshaded areas have no record in this dataset; they do not prove absence.
Source: Kew species record · WCVP, version 16 (June 2026), Royal Botanic Gardens, Kew, CC BY 3.0. Map boundaries: TDWG / WGSRPD; adapted to a world map.
Measured properties
Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.
- Janka hardness
- 510 lbf
- Density at 12% MC
- 32.2 lb/ft³
- Specific gravity
- 0.46
- Modulus of rupture
- 11,900 lb/in²
- Modulus of elasticity
- 1.49 ×10⁶ lb/in²
- Crushing strength
- 6,230 lb/in²
- Radial shrinkage
- No published test
- Tangential shrinkage
- No published test
- Volumetric shrinkage
- No published test
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Where these numbers come from
Check the references below to see which properties each source supports.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Janka hardness · Green wood hardness · Specific gravity · Basic specific gravity · Density · Bending strength · Stiffness · Crushing strength · Green wood properties
- manual map (regional variant)
Scientific name
- GWDD v2.2 (Fischer et al. 2026)
Botanical family
Interior South Douglas-fir wood: a practical guide
Interior South Douglas-fir (Pseudotsuga menziesii) is listed as a softwood from North America. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.
Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.
What is Interior South Douglas-fir?
The botanical name used by this record is Pseudotsuga menziesii, in the Pinaceae family. When buying, ask the supplier to identify the species rather than relying on the common name alone.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Pseudotsuga menziesii
The range of Douglas-fir extends from the Rocky Mountains to the Pacific Coast and from Mexico to central British Columbia. The Douglas-fir production comes from the Coast States of Oregon, Washington, and California, and the Rocky Mountain States.
Common names can vary between countries and suppliers. For a restoration, repeat order, or technical specification, keep the botanical name and the supplier’s description with the material record.
A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.
General workshop reference: USDA Wood Handbook (public domain)
Color, grain, and choosing visible boards
The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Pseudotsuga menziesii
The wood of Douglas-fir varies widely in weight and strength. The sapwood of Douglas-fir is narrow in old-growth trees but can be as much as 3 in. (7.62 cm) wide in second-growth trees of commercial size. Young trees of moderate to rapid growth have reddish heartwood and are called red-fir. Very narrow-ringed wood of old trees may be yellowish brown and is known on the market as yellow-fir.
For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.
- Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
- Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
- Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.
General workshop reference: USDA Wood Handbook (public domain)
Hardness, weight, and strength in practice
Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.
- Janka hardness: 510 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Density: 32.2 lb/ft³.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Bending strength: 11,900 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Stiffness: 1.49 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
- Compression parallel to grain: 6,230 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
Uses and project selection for Interior South Douglas-fir
The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Pseudotsuga menziesii
Douglas-fir is used mostly for building and construction purposes in the form of lumber, timbers, piles, and plywood. Considerable quantities go into cooperage stock, mine timbers, poles, and fencing. Douglas-fir lumber is used in the manufacture of various products, including sash, doors, laminated beams, general millwork, boxes, pallets, and crates. Small amounts are used for flooring, furniture, ship and boat construction, and tanks. Douglas-fir plywood has found ever-increasing usefulness in construction, furniture, cabinets, and many other products.
Allow for visible dents on a heavily used surface. This hardness may be workable for many interior parts, but a tabletop or floor also needs a suitable finish and a realistic maintenance plan.
Based on the recorded density, calculate the weight of the finished volume before choosing hardware or building a portable piece. Moisture content and individual boards can change the result.
- Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
- Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
- Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
- Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.
General workshop reference: USDA Wood Handbook (public domain)
Sawing, planing, routing, and drilling
Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Pseudotsuga menziesii
Douglas-fir wood is strong, moderately hard, and very stiff. It is rather difficult to work with using hand tools, splits easily, but has good machining properties.
- Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
- Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
- Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
- Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
- Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
- Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.
General workshop reference: USDA Wood Handbook (public domain)
Drying, shrinkage, and seasonal movement
No shrinkage figures are available in this record. That is missing evidence, not proof of low movement.
Shrinkage is not documented in this record. For wide solid parts, ask for drying history and movement data or use a construction that does not depend on an unverified stability claim.
Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.
- Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
- Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
- Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.
General workshop reference: USDA Wood Handbook (public domain)
Gluing and assembly
Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.
A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.
Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.
General workshop reference: USDA Wood Handbook (public domain)
Finishing, staining, and surface preparation
Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.
Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.
- Prepare consistently: remove marks from each sanding stage and inspect under raking light.
- Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
- Include end grain: test it when it will remain visible, since it can take color differently from the face.
- Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.
General workshop reference: USDA Wood Handbook (public domain)
Decay resistance, exposure, and care
Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.
Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain
Source profile: Pseudotsuga menziesii
The heartwood is moderately resistant to decay.
For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.
For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.
General workshop reference: USDA Wood Handbook (public domain)
Buying Interior South Douglas-fir: a practical checklist
Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.
For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.
- Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
- Moisture: ask about drying history and check the stock against the intended application.
- Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
- Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
- Specification: obtain appropriate grade or product evidence for structural or demanding service.
- Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.
General workshop reference: USDA Wood Handbook (public domain)
Dust, food contact, and care
The occupational-source record linked to Interior South Douglas-fir reports bronchial effects, dermatitis, rhinitis, splinters go septic. The botanical name matched the source entry, so this record is about this species.
Read the reported effects, source evidence, and match confidence for Interior South Douglas-fir.
For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.
- Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
- Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
- Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.
Comparing alternatives
The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.
| Wood | Janka | Density |
|---|---|---|
| Interior South Douglas-firPseudotsuga menziesii | 510 lbf | 32.2 lb/ft³ |
| Coast Douglas-firPseudotsuga menziesii | 710 lbf | 33.6 lb/ft³ |
| Interior North Douglas-firPseudotsuga menziesii | 600 lbf | 33.6 lb/ft³ |
| Interior West Douglas-firPseudotsuga menziesii | 660 lbf | 35.0 lb/ft³ |
Before you build
- Confirm the species and the usable dimensions of the stock.
- Check the properties that matter to the part, including any estimates or gaps.
- Match moisture to the intended environment and allow cross-grain movement.
- Make representative cutting, bonding, and finishing trials.
- Keep the approved sample, product details, and care instructions with the job.
Sources and further reading
Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.
- Alden — Softwoods of North America (1997), FPL-GTR-102
Pseudotsuga menziesii · species description · public domain. Historical species descriptions. Nursery, medicinal, and industrial uses mentioned by the source are not instructions for making a product.
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
public domain. Supports: janka lbf, janka n, janka green lbf, specific gravity 12, specific gravity basic, density kg m3, mor psi, moe mpsi, crushing psi, green.
- manual map (regional variant)
public domain. Supports: scientific name.
- GWDD v2.2 (Fischer et al. 2026)
CC BY 4.0. Supports: family.
- USDA FPL — Wood Handbook (2021)
Public domain. Chapters on moisture, mechanical properties, fastenings, design, bonding, drying, decay, preservation, and finishing provide the general workshop background.
- USDA FSIS — Cutting Boards
Public domain. Cleaning, cross-contamination prevention, and board replacement.
Compare before you choose
See how Interior South Douglas-fir and Coast Douglas-fir differ in hardness, density, strength, and shrinkage, with sources alongside the values.
Compare Interior South Douglas-fir with Coast Douglas-firHealth and safety
A published occupational source reports bronchial effects, dermatitis, rhinitis, splinters go septic for this wood. What that means, and how strong the link is.
Woods of similar hardness
A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.
| # | Wood | Janka | |
|---|---|---|---|
| 1 | Baldcypress | 510 lbf | |
| 2 | Banak | 510 lbf | |
| 3 | Sitka spruce | 510 lbf | |
| 4 | Black poplar | 509 lbf* | |
| 5 | Chinese catalpa | 509 lbf* | |
| 6 | Chuchab | 509 lbf* |