Wood Record

Tropical America · hardwood

Sucupira

Diplotropis purpurea, Fabaceae

Also sold as: Botonallare, Peonía, Tatabu, Aramatta, Zwarte kabbes, Coeur dehors, Sapupira, Supupira

Read the practical guide to Sucupira

Janka hardness

2,140 lbf

Harder than 79% of the 571 species with a laboratory test.

At a glance

Janka hardness
2,140 lbf
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density
56.2 lb/ft³
LPF/SFB Madeiras Brasileiras
Volumetric shrinkage
11.8%
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Availability · editorial
Rarely traded

Working characteristics: The wood is moderately difficult to work and resulting surfaces, especially in planing, are fair to poor due to the coarse texture and frequent grain irregularity. Chudnoff — Tropical Timbers of the World (1984), AH-607

Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.

Sourced wood and tree images

Each image names its author, its licence, and the page it came from.

Geographic distribution

Where it grows

NativeIntroducedNo record

Recorded distribution of Diplotropis purpurea. Native areas are part of its natural range; introduced areas are places where it has been brought by people.

Loading world map…

Explore native and introduced regions

Native range (11 regions)

Bolivia · Brazil North · Brazil Northeast · Brazil West-Central · Colombia · Ecuador · French Guiana · Guyana · Peru · Surinam · Venezuela

Introduced range (0 regions)

No regions recorded in this dataset.

Shading marks botanical regions with recorded presence, not the exact extent of forests or commercial plantations. Large countries may be divided into states or provinces. Extinct and doubtful records are excluded. Unshaded areas have no record in this dataset; they do not prove absence.

Source: Kew species record · WCVP, version 16 (June 2026), Royal Botanic Gardens, Kew, CC BY 3.0. Map boundaries: TDWG / WGSRPD; adapted to a world map.

Measured properties

Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.

Janka hardness
2,140 lbf

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Density at 12% MC
56.2 lb/ft³

LPF/SFB Madeiras Brasileiras

Specific gravityestimate
0.89

USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

Modulus of rupture
20,600 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Modulus of elasticity
2.87 ×10⁶ lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Crushing strength
12,140 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Radial shrinkage
4.6%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

Tangential shrinkage
7.0%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

Volumetric shrinkage
11.8%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

Where these numbers come from

Check the references below to see which properties each source supports.

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

    Janka hardness · Green wood hardness · Basic specific gravity · Bending strength · Stiffness · Crushing strength · Green wood properties

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

    Shrinkage

  • LPF/SFB Madeiras Brasileiras

    Botanical family · Density

  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

    Specific gravity

One value on this page is an estimate. Estimates use the specific-gravity conversions or regressions identified in the source records. An estimate is not a test result. Each one carries a mark.

Sucupira wood: a practical guide

Sucupira (Diplotropis purpurea) is listed as a hardwood from Tropical America. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.

Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.

What is Sucupira?

The botanical name used by this record is Diplotropis purpurea, in the Fabaceae family. Other names recorded here include Botonallare, Peonía, Tatabu, Aramatta, Zwarte kabbes, Coeur dehors, Sapupira, Supupira.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Source profile: Diplotropis purpurea

Uplands of the Guianas and in Para and Amazonas in Brazil. Fairly common in parts of Brazil and French Guiana, infrequent in Surinam and Guyana.

Common names can vary between countries and suppliers. For a restoration, repeat order, or technical specification, keep the botanical name and the supplier’s description with the material record.

A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.

General workshop reference: USDA Wood Handbook (public domain)

Color, grain, and choosing visible boards

The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Source profile: Diplotropis purpurea

Freshly cut heartwood is generally chocolate brown turning to a lighter brown when dry, occasionally grayish brown, with fine lighter parenchyma stripes; sharply demarcated from whitish or yellowish sapwood. Texture coarse; grain usually straight to slightly interlocked or slightly wavy; luster medium to high and golden, often with a waxy appearance; without distinctive odor or taste.

Translated test-lot description · Brazilian Forest Service / LPF — Madeiras Brasileiras · CC BY 4.0

Source profile: Diplotropis purpurea

The LPF test-lot descriptions report: Heartwood color: brown. Texture: medium. Grain: interlocked.

For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.

  • Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
  • Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
  • Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.

General workshop reference: USDA Wood Handbook (public domain)

Hardness, weight, and strength in practice

Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.

  • Janka hardness: 2,140 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Density: 56.2 lb/ft³.Source: LPF/SFB Madeiras Brasileiras (CC BY 4.0).
  • Bending strength: 20,600 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Stiffness: 2.87 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Compression parallel to grain: 12,140 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).

Property sources and licences

Uses and project selection for Sucupira

The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Source profile: Diplotropis purpurea

Heavy construction work, boat building, flooring, furniture components, turnery, railroad crossties, and tool handles.

Surface hardness is a reason to compare this wood for wear, while allowing for greater cutting effort. Make trial cuts and pilot holes before machining or fastening the finished parts.

Based on the recorded density, weight deserves early attention for a large top, door, or portable object. Include the base, hardware, and lifting requirements in the design.

  • Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
  • Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
  • Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
  • Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.

General workshop reference: USDA Wood Handbook (public domain)

Sawing, planing, routing, and drilling

Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Source profile: Diplotropis purpurea

The wood is moderately difficult to work and resulting surfaces, especially in planing, are fair to poor due to the coarse texture and frequent grain irregularity.
  • Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
  • Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
  • Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
  • Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
  • Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
  • Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.

General workshop reference: USDA Wood Handbook (public domain)

Drying, shrinkage, and seasonal movement

Recorded green-to-ovendry shrinkage: radial 4.6%; tangential 7.0%; volumetric 11.8%. Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.

Tangential shrinkage is about 1.5 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.

Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.

  • Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
  • Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
  • Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.

General workshop reference: USDA Wood Handbook (public domain)

Gluing and assembly

Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.

A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.

Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.

General workshop reference: USDA Wood Handbook (public domain)

Finishing, staining, and surface preparation

Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.

Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.

  • Prepare consistently: remove marks from each sanding stage and inspect under raking light.
  • Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
  • Include end grain: test it when it will remain visible, since it can take color differently from the face.
  • Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.

General workshop reference: USDA Wood Handbook (public domain)

Decay resistance, exposure, and care

Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Source profile: Diplotropis purpurea

In laboratory evaluations, the heartwood is rated very durable in resistance to both white-rot and brown-rot fungi. Other evaluations rate the wood as moderately durable; highly resistant to attack by dry-wood termites; not resistant to marine borers.

For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.

For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.

General workshop reference: USDA Wood Handbook (public domain)

Buying Sucupira: a practical checklist

Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.

For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.

  • Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
  • Moisture: ask about drying history and check the stock against the intended application.
  • Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
  • Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
  • Specification: obtain appropriate grade or product evidence for structural or demanding service.
  • Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.

General workshop reference: USDA Wood Handbook (public domain)

Dust, food contact, and care

The dedicated occupational-source dataset has no reaction report linked to this entry. Historical descriptions may discuss additional handling concerns. An absent report does not establish that dust is harmless or that the wood is suitable for food contact. Use appropriate dust control and follow the controls for the tools and materials you use.

For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.

  • Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
  • Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
  • Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.

USDA FSIS: Cutting Boards (public domain) · HSE: Wood dust

Comparing alternatives

The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.

Comparison choices are editorial, prioritizing related and commonly traded woods with measured hardness. Estimates are labelled; a dash means no recorded value. Each species links to its full sources.
WoodJankaDensity
SucupiraDiplotropis purpurea2,140 lbf56.2 lb/ft³
CanaleteCordia spp. (hard-wooded, dark-colored Gerascanthus group)2,200 lbf58.2 lb/ft³Estimate
PurpleheartPeltogyne spp.1,860 lbf58.0 lb/ft³
Mockernut hickoryCarya alba1,970 lbf50.3 lb/ft³

Before you build

  1. Confirm the species and the usable dimensions of the stock.
  2. Check the properties that matter to the part, including any estimates or gaps.
  3. Match moisture to the intended environment and allow cross-grain movement.
  4. Make representative cutting, bonding, and finishing trials.
  5. Keep the approved sample, product details, and care instructions with the job.

Sources and further reading

Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.

Compare before you choose

See how Sucupira and Canalete differ in hardness, density, strength, and shrinkage, with sources alongside the values.

Compare Sucupira with Canalete

Woods of similar hardness

A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.

#WoodJanka
1Danta2,140 lbf
2Pignut hickory2,140 lbf
3Akee2,139 lbf*
4Black mangrove2,139 lbf*
5Bois bande2,139 lbf*
6Burkea2,139 lbf*

All species