Wood Record

Asia · hardwood

Light red meranti

Shorea spp., Dipterocarpaceae

Read the practical guide to Light red meranti

Janka hardness

460 lbf

Harder than 7% of the 571 species with a laboratory test.

At a glance

Janka hardness
460 lbf
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density
25.1 lb/ft³ · estimate
USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Volumetric shrinkage
No published value
Availability · editorial
Rarely traded

Working characteristics need separate confirmation; this record has no species-specific published description.

Missing evidence: shrinkage, species-specific working description, species-specific durability description.

Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.

Sourced wood and tree images

No species-specific open-licence image was found in our current sources. These show other species of Shorea. A sample of the genus is a guide to colour and grain, not a record of this wood.

Geographic distribution

Where it grows

A reliable species-level range is not yet available for this record. Some wood names cover several species, and some scientific names need further verification. We’ll add a map when the name can be matched to a documented distribution.

Measured properties

Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.

Janka hardness
460 lbf

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Density at 12% MCestimate
25.1 lb/ft³

USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

Specific gravityestimate
0.36

USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

Modulus of rupture
9,500 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Modulus of elasticity
1.23 ×10⁶ lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Crushing strength
5,920 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

Radial shrinkage
No published test
Tangential shrinkage
No published test
Volumetric shrinkage
No published test

Where these numbers come from

Check the references below to see which properties each source supports.

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b

    Janka hardness · Green wood hardness · Basic specific gravity · Bending strength · Stiffness · Crushing strength · Green wood properties

  • GWDD v2.2 (Fischer et al. 2026)

    Botanical family

  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9

    Specific gravity · Density

2 values on this page are estimates. Estimates use the specific-gravity conversions or regressions identified in the source records. An estimate is not a test result. Each one carries a mark.

Light red meranti wood: a practical guide

Light red meranti (Shorea spp.) is listed as a hardwood from Asia. The available descriptive evidence concerns a broader group; the scope is identified beside each source passage. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.

Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.

What is Light red meranti?

The botanical name used by this record is Shorea spp., in the Dipterocarpaceae family. When buying, ask the supplier to identify the species rather than relying on the common name alone.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Malay Peninsula including Indochina, Indonesia, Philippines; often in almost pure stands.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Malaysia, Indonesia, and the Philippines.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Malay Peninsula, Indonesia, the Philippines, as well as Sabah and Sarawak, usually at low altitudes on well-drained soils.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Widely distributed from India in the north and west through the Malayan Peninsula to the Philippines and Celebes to the east.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Malaysia, Indonesia, and the Philippines.

The botanical label represents a group rather than a single identified species. Material sold under it may include different species, and a property reported for that group is not a guarantee for every board.

A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.

General workshop reference: USDA Wood Handbook (public domain)

Color, grain, and choosing visible boards

The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood dark brown, medium to deep red, sometimes with a purplish tinge, commonly with white dammar or resin streaks; sapwood pinkish, rather poorly defined. Texture rather coarse; grain interlocked, sometimes straight; luster low, without characteristic odor or taste.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood variable from almost white to pale pink to dark red, or pale brown to deep brown; sapwood lighter usually with a grayish tinge, distinct. Grain usually interlocked, sometimes somewhat straight; texture coarse; slightly lustrous; usually without characteristic odor or taste.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood whitish when freshly cut, becoming light yellow brown on exposure; sapwood about 2 to 2.5 in. wide, poorly defined. Texture moderately coarse and even; grain interlocked; slightly lustrous; dried material without characteristic odor or taste. Silica is abundant in the ray tissue.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood light yellow or yellow brown, sometimes with a greenish tinge, darkening on exposure; sapwood paler in color, often with a grayish tinge. Texture moderately coarse; grain shallowly interlocked; luster low, dry material without characteristic odor or taste; liable to discolor if in contact with iron under moist conditions.

For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.

  • Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
  • Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
  • Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.

General workshop reference: USDA Wood Handbook (public domain)

Hardness, weight, and strength in practice

Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.

  • Janka hardness: 460 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Density: 25.1 lb/ft³ — an estimate, not a laboratory test.Source: USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 (public domain).
  • Bending strength: 9,500 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Stiffness: 1.23 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).
  • Compression parallel to grain: 5,920 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b (public domain).

Property sources and licences

Uses and project selection for Light red meranti

The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heavy construction, framing of boats, parquet flooring, heavy-duty flooring, utility furniture.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Veneer and plywood, joinery, flooring, furniture and cabinetwork, general construction, boatbuilding.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Light structural work, furniture components, joinery, plywood, cabinetwork, flooring, concrete form work, a general utility wood.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Veneer and plywood, flooring, general construction, vats and casks, boat framing.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Joinery, flooring, furniture components, plywood, paneling, light structural work. Dammar exudates are collected from trees in Malaya.

The measured hardness is below that of many furniture hardwoods. Prioritize protection from dents and generous bearing areas beneath fasteners; consider whether the project needs a harder wearing surface.

Based on the estimated density, handling weight may be an advantage for larger parts. Check the actual stock and design connections for its properties rather than substituting dimensions from a heavier wood.

  • Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
  • Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
  • Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
  • Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.

General workshop reference: USDA Wood Handbook (public domain)

Sawing, planing, routing, and drilling

Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Rather difficult to machine because of high density, saws cleanly, dresses to a smooth finish, some tearing of interlocked grain, only moderate blunting of cutters, wood should be prebored for nailing.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Easy to work with hand and machine tools, dresses to a smooth finish, some tearing of interlocked grain; good gluing and nailing properties; takes a good finish.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Easy to work with both hand and machine tools; nailing and gluing are satisfactory; takes a good finish, resin and oil exudation is not a problem.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Very difficult to saw or machine due to rapid dulling of cutters caused by high silica content; stellite-tipped or carbide-tipped tools are suggested; sawn surfaces tend to be woolly.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Works easily with hand and machine tools and dresses to a smooth finish, some tearing of interlocked grain; good gluing and nailing characteristics; suitable for steam bending to a moderate radius of curvature.
  • Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
  • Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
  • Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
  • Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
  • Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
  • Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.

General workshop reference: USDA Wood Handbook (public domain)

Drying, shrinkage, and seasonal movement

No shrinkage figures are available in this record. That is missing evidence, not proof of low movement.

Shrinkage is not documented in this record. For wide solid parts, ask for drying history and movement data or use a construction that does not depend on an unverified stability claim.

Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.

  • Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
  • Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
  • Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.

General workshop reference: USDA Wood Handbook (public domain)

Gluing and assembly

Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.

A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.

Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.

General workshop reference: USDA Wood Handbook (public domain)

Finishing, staining, and surface preparation

Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.

Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.

  • Prepare consistently: remove marks from each sanding stage and inspect under raking light.
  • Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
  • Include end grain: test it when it will remain visible, since it can take color differently from the face.
  • Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.

General workshop reference: USDA Wood Handbook (public domain)

Decay resistance, exposure, and care

Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood durability very variable and should be classified as nondurable. Sapwood is very susceptible to attack by powder-post beetle.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood is rated as only moderately durable and should not be used in high hazard areas; sapwood liable to attack by powder-post beetles. Not resistant to marine borers.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood generally rated as nondurable in ground contact and is susceptible to dry-wood and subterranean termite attack; sapwood liable to powder-post beetle attack.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Not durable in ground contact and vulnerable to dry-wood and subterranean termite attack. Though silica content is high, there is no immunity to marine borer attack.

Historical source excerpt · Chudnoff — Tropical Timbers of the World (1984), AH-607 · public domain

Group profile: Shorea spp. This passage can describe several species; traits and uses do not necessarily apply to every member.

Heartwood not durable in exposed conditions or in ground contact, liable to termite attack. Sapwood susceptible to powder-post beetle attack. Not resistant to marine borers.

For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.

For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.

General workshop reference: USDA Wood Handbook (public domain)

Buying Light red meranti: a practical checklist

Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.

For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.

  • Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
  • Moisture: ask about drying history and check the stock against the intended application.
  • Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
  • Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
  • Specification: obtain appropriate grade or product evidence for structural or demanding service.
  • Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.

General workshop reference: USDA Wood Handbook (public domain)

Dust, food contact, and care

The occupational-source record linked to Light red meranti reports skin irritation. A source entry for the genus matched. The report belongs to the genus, and this species may differ from its relatives.

Read the reported effects, source evidence, and match confidence for Light red meranti.

For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.

  • Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
  • Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
  • Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.

USDA FSIS: Cutting Boards (public domain) · HSE: Wood dust

Comparing alternatives

The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.

Comparison choices are editorial, prioritizing related and commonly traded woods with measured hardness. Estimates are labelled; a dash means no recorded value. Each species links to its full sources.
WoodJankaDensity
Light red merantiShorea spp.460 lbf25.1 lb/ft³Estimate
Yellow merantiShorea spp.770 lbf34.7 lb/ft³Estimate
Dark red merantiShorea spp.780 lbf53.0 lb/ft³
White merantiShorea spp.1,140 lbf42.1 lb/ft³Estimate

Before you build

  1. Confirm the species and the usable dimensions of the stock.
  2. Check the properties that matter to the part, including any estimates or gaps.
  3. Match moisture to the intended environment and allow cross-grain movement.
  4. Make representative cutting, bonding, and finishing trials.
  5. Keep the approved sample, product details, and care instructions with the job.

Sources and further reading

Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.

Compare before you choose

See how Light red meranti and Yellow meranti differ in hardness, density, strength, and shrinkage, with sources alongside the values.

Compare Light red meranti with Yellow meranti

Health and safety

A published occupational source reports skin irritation for this wood. What that means, and how strong the link is.

Woods of similar hardness

A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.

#WoodJanka
1Mexican cypress460 lbf
2Ponderosa pine460 lbf
3Pulai460 lbf
4Magas462 lbf
5Fava-bolota / visgueiro463 lbf
6Marupá452 lbf

All species