Wood Record

North America · softwood

Red spruce

Picea rubens, Pinaceae

Read the practical guide to Red spruce

Janka hardness

530 lbf

Harder than 11% of the 571 species with a laboratory test.

At a glance

Janka hardness
530 lbf
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Density
28.0 lb/ft³
USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b
Volumetric shrinkage
11.8%
USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3
Availability · editorial
Widely stocked

Working characteristics: It is easily worked, glues well, has average paint-holding ability, and low nail-holding capacity. Alden — Softwoods of North America (1997), FPL-GTR-102

Shrinkage is green to ovendry, not seasonal movement. Availability is an editorial guide, not a stock check.

Sourced wood and tree images

Each image names its author, its licence, and the page it came from.

Geographic distribution

Where it grows

NativeIntroducedNo record

Recorded distribution of Picea rubens. Native areas are part of its natural range; introduced areas are places where it has been brought by people.

Loading world map…

Explore native and introduced regions

Native range (19 regions)

Connecticut · Maine · Maryland · Massachusetts · New Brunswick · New Hampshire · New Jersey · New York · Newfoundland · North Carolina · Nova Scotia · Ontario · Pennsylvania · Prince Edward I. · Québec · Tennessee · Vermont · Virginia · West Virginia

Introduced range (0 regions)

No regions recorded in this dataset.

Shading marks botanical regions with recorded presence, not the exact extent of forests or commercial plantations. Large countries may be divided into states or provinces. Extinct and doubtful records are excluded. Unshaded areas have no record in this dataset; they do not prove absence.

Source: Kew species record · WCVP, version 16 (June 2026), Royal Botanic Gardens, Kew, CC BY 3.0. Map boundaries: TDWG / WGSRPD; adapted to a world map.

Measured properties

Dry-wood properties are shown for comparison; published moisture conditions can differ between sources. Shrinkage is from green to ovendry, not seasonal movement. Actual properties in service vary.

Janka hardness
530 lbf

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Density at 12% MC
28.0 lb/ft³

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Specific gravity
0.40

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Modulus of rupture
10,800 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Modulus of elasticity
1.66 ×10⁶ lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Crushing strength
5,540 lb/in²

USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

Radial shrinkage
3.8%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3

Tangential shrinkage
7.8%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3

Volumetric shrinkage
11.8%

USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3

Where these numbers come from

Check the references below to see which properties each source supports.

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b

    Janka hardness · Green wood hardness · Specific gravity · Basic specific gravity · Density · Bending strength · Stiffness · Crushing strength · Green wood properties

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3

    Shrinkage

  • USDA FIA REF_SPECIES

    Scientific name

  • GWDD v2.2 (Fischer et al. 2026)

    Botanical family

Red spruce wood: a practical guide

Red spruce (Picea rubens) is listed as a softwood from North America. The source descriptions below explain its appearance, working characteristics, and documented uses where those have been published. Use this guide to connect that evidence to buying stock, choosing a project, and planning the work.

Species and group descriptions are attributed below. Practical recommendations explain how to use the available evidence; they are editorial guidance. Estimates and missing properties remain identified. Historical uses describe the source’s publication period.

What is Red spruce?

The botanical name used by this record is Picea rubens, in the Pinaceae family. When buying, ask the supplier to identify the species rather than relying on the common name alone.

Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain

Source profile: Picea rubens

Red spruce is native to Cape Breton Islands, Nova Scotia, and New Brunswick, west to Maine, southern Quebec, and southeastern Ontario and south to central New York, northeastern Pennsylvania, northern New Jersey, and Massachusetts. It also grows in the Appalachian Mountains of extreme western Maryland, eastern West Virginia, northern and western Virginia, western North Carolina, and eastern Tennessee.

Common names can vary between countries and suppliers. For a restoration, repeat order, or technical specification, keep the botanical name and the supplier’s description with the material record.

A broad region describes this database entry, not the origin of the board offered for sale. Verify the shipment’s origin and sourcing documents if these affect your purchase. A description in an older timber reference also does not establish present-day availability.

General workshop reference: USDA Wood Handbook (public domain)

Color, grain, and choosing visible boards

The attributed descriptions below are a starting point for recognizing color and grain. Compare them with clean, freshly surfaced stock; oxidation, drying, lighting, and a coating can all change what a sample looks like.

Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain

Source profile: Picea rubens

The wood dries easily and is stable after drying, is moderately light in weight and easily worked, has moderate shrinkage, and is moderately strong, stiff, tough, and hard. It is not very resistant to bending or end-wise compression. It is straight, even grained, medium to fine textured, soft, and produces a lustrous finish. It is without characteristic odor or taste. The wood is a pale yellowish white, and there is little difference in color between the heartwood and sapwood. It has exceptional resonance qualities, in the form of thin boards. It has moderately high shrinkage, but is easily air or kiln dried.

For visible work, buy the boards as a set. Decide whether changes between sapwood and heartwood are welcome, and lay out adjacent parts before cutting. A small attractive sample may not show the range of color or figure in a full order.

  • Color match: evaluate the actual faces that will be visible, with the intended finish on a spare piece.
  • Grain direction: follow the fibers through narrow parts, joints, and curved shapes; decorative figure can complicate cutting.
  • Soundness: check both ends and faces for splits, decay, loose knots, and defects that reduce usable length.

General workshop reference: USDA Wood Handbook (public domain)

Hardness, weight, and strength in practice

Each property answers a different question. Janka side hardness compares indentation resistance, density helps with handling weight, stiffness relates to deflection, and bending strength concerns failure. None can stand in for all the others.

  • Janka hardness: 530 lbf.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
  • Density: 28.0 lb/ft³.Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
  • Bending strength: 10,800 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
  • Stiffness: 1.66 ×10⁶ lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).
  • Compression parallel to grain: 5,540 lb/in².Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-3b (public domain).

Property sources and licences

Uses and project selection for Red spruce

The source’s use list records applications reported when that reference was compiled. It can suggest where the material has been useful, but each finished product still needs stock, construction, and specifications suited to the job.

Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain

Source profile: Picea rubens

The largest use of red spruce is pulpwood. It is also used for framing material, general millwork, boxes and crates, and piano sounding boards.

Allow for visible dents on a heavily used surface. This hardness may be workable for many interior parts, but a tabletop or floor also needs a suitable finish and a realistic maintenance plan.

Based on the recorded density, handling weight may be an advantage for larger parts. Check the actual stock and design connections for its properties rather than substituting dimensions from a heavier wood.

  • Furniture and cabinetry: check visible color, grain at joints, stiffness for spans, and room for solid panels to move.
  • Wear surfaces: compare measured hardness and the complete flooring or worktop specification, including coating and maintenance.
  • Small turned or carved objects: inspect the blank’s soundness and make a cutting trial before choosing a thin profile.
  • Outdoor or wet service: require decay-resistance and exposure evidence, together with drainage, hardware, and treatment details where applicable.

General workshop reference: USDA Wood Handbook (public domain)

Sawing, planing, routing, and drilling

Use the published working description below to plan the first trial. The following steps are general workshop recommendations; they are not a tested feed-rate schedule for this species.

Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain

Source profile: Picea rubens

It is easily worked, glues well, has average paint-holding ability, and low nail-holding capacity.
  • Start with sound stock: locate checks, short grain, and other defects before holding the work or setting the cut.
  • Plane a trial face: read the grain and begin with a light pass. If grain reverses or tears, adjust the cut and consider scraping or sanding rather than repeatedly cutting deeper.
  • Check heat and rubbing: sharp, clean cutters and a suitable feed help. Investigate burn marks instead of forcing a cut; follow the machine and cutter instructions.
  • Back up exit edges: use suitable support when drilling or machining joints to reduce breakout. Trial-fit joinery before glue-up.
  • Test fasteners: size pilot and clearance holes for the actual screw and stock. Dense material may split near an end, while softer material may crush beneath a fastener.
  • Inspect the surface: use raking light to find machining marks, sanding scratches, and glue contamination before coating.

General workshop reference: USDA Wood Handbook (public domain)

Drying, shrinkage, and seasonal movement

Recorded green-to-ovendry shrinkage: radial 3.8%; tangential 7.8%; volumetric 11.8%. Source: USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-3 (public domain). These describe drying over a much wider moisture range than a typical finished interior piece experiences.

Tangential shrinkage is about 2.1 times radial shrinkage, calculated from the published values. Growth-ring orientation therefore belongs in the selection of a wide panel. The ratio describes directional differences; it does not measure the total seasonal movement or prove that a board will remain flat.

Bring stock close to the conditions in which the finished object will live before final sizing and assembly. Check moisture with a meter used according to its instructions and the appropriate species correction. Kiln-dried does not mean that the wood is at the right moisture content for every room or climate.

  • Wide tops: choose attachments that permit cross-grain movement, such as correctly installed clips or screws in appropriately oriented slots.
  • Frame-and-panel work: allow the panel to move within the frame, following the chosen construction method.
  • Freshly sawn lumber: use a drying schedule appropriate to the material and thickness; the shrinkage table is not a kiln schedule.

General workshop reference: USDA Wood Handbook (public domain)

Gluing and assembly

Prepare sound, properly fitted surfaces and make a complete dry assembly before spreading glue. Choose an adhesive for the intended exposure and follow its requirements for moisture, temperature, open time, pressure, and cure.

A species description that mentions natural oils, extractives, or difficult bonding is a reason to verify the adhesive system on the actual stock. Do not assume that sanding finer or wiping with an arbitrary solvent will solve an adhesion problem. Use the adhesive manufacturer’s preparation guidance.

Clamp pressure should close a well-made joint. If it takes excessive force to bring the pieces together dry, correct the fit or the stock first. Remove glue contamination before finishing and check corners, shoulders, and exposed end grain.

General workshop reference: USDA Wood Handbook (public domain)

Finishing, staining, and surface preparation

Choose the finish for the object’s use and the appearance you want. A clear coating reveals natural variation; a stain can emphasize differences in absorption. A decorative object, dining table, and exterior component need different protection and maintenance.

Do not infer finishing behavior from color or density alone. Open pores may influence the desired surface texture, while uneven absorption may complicate a uniform stain. Confirm the treatment on an offcut rather than selecting a pore filler, conditioner, or sealer by habit.

  • Prepare consistently: remove marks from each sanding stage and inspect under raking light.
  • Sample the whole system: reproduce the sanding, any color treatment, and the topcoat on stock from the project.
  • Include end grain: test it when it will remain visible, since it can take color differently from the face.
  • Check the result in use: allow the sample to dry and cure as directed, then examine it in the intended lighting.

General workshop reference: USDA Wood Handbook (public domain)

Decay resistance, exposure, and care

Read the source’s durability statement with its scope in mind. Heartwood, sapwood, resistance to a particular insect, and performance in a particular test are different things. An older durability report is useful background, not a service-life warranty.

Historical source excerpt · Alden — Softwoods of North America (1997), FPL-GTR-102 · public domain

Source profile: Picea rubens

The heartwood of spruce is slightly resistant to nonresistant to decay.

For interior pieces, follow the coating’s cleaning instructions and deal with spills promptly. Persistent dampness, trapped water at joints, and an unsuitable indoor humidity range need attention even when the surface appears well finished.

For exterior work, choose a documented material or product for the exposure. Provide drainage, avoid water-trapping pockets, and use compatible hardware. Ground contact and marine exposure demand more than a general statement that a timber is durable.

General workshop reference: USDA Wood Handbook (public domain)

Buying Red spruce: a practical checklist

Price depends on the usable stock, not just a species name. Thickness, clear lengths, figure, color selection, drying, surfacing, quantity, and supply all affect the value of a quote. Compare like-for-like dimensions and include machining waste.

For an unfamiliar species or a large order, start with a sample and a small trial. Keep the supplier’s identification, stock condition, and sourcing information with the job so you can explain or repeat the choice later.

  • Identity: confirm the botanical name and whether the shipment is a mixture or a single species.
  • Moisture: ask about drying history and check the stock against the intended application.
  • Usable dimensions: allow for flattening, trimming, checks, knots, and defects around the parts you need.
  • Appearance: inspect the actual lot together if matching pale faces, heartwood color, or figure matters.
  • Specification: obtain appropriate grade or product evidence for structural or demanding service.
  • Supply and origin: check the actual shipment’s documentation; a reference-book entry does not prove current availability or permission to trade.

General workshop reference: USDA Wood Handbook (public domain)

Dust, food contact, and care

The occupational-source record linked to Red spruce reports photosensitisation, respiratory disorders. A source entry for the genus matched. The report belongs to the genus, and this species may differ from its relatives.

Read the reported effects, source evidence, and match confidence for Red spruce.

For a cutting board, utensil, or other food-contact object, confirm the material’s identity and history separately from its hardness. Unknown treatments, coatings, decay, and hard-to-clean defects can rule out a piece that otherwise looks attractive.

  • Adhesive and finish: select products intended for the application and observe the manufacturer’s curing instructions.
  • Cleaning: USDA advises washing cutting boards with hot, soapy water, rinsing, and drying after use. Keep raw-meat preparation separate from ready-to-eat foods.
  • Condition: replace cutting boards when wear or grooves make them difficult to clean. Follow the care instructions for the construction; laminated boards can split in a dishwasher.

USDA FSIS: Cutting Boards (public domain) · HSE: Wood dust

Comparing alternatives

The nearby measured-hardness values below help put dent resistance in context. Use appearance, movement, machining, supply, and exposure evidence to decide whether a different species is a practical substitute.

Comparison choices are editorial, prioritizing related and commonly traded woods with measured hardness. Estimates are labelled; a dash means no recorded value. Each species links to its full sources.
WoodJankaDensity
Red sprucePicea rubens530 lbf28.0 lb/ft³
Black sprucePicea mariana530 lbf29.3 lb/ft³
Sitka sprucePicea sitchensis510 lbf28.0 lb/ft³
White sprucePicea glauca410 lbf25.2 lb/ft³

Before you build

  1. Confirm the species and the usable dimensions of the stock.
  2. Check the properties that matter to the part, including any estimates or gaps.
  3. Match moisture to the intended environment and allow cross-grain movement.
  4. Make representative cutting, bonding, and finishing trials.
  5. Keep the approved sample, product details, and care instructions with the job.

Sources and further reading

Quoted descriptions retain the source’s scope and historical context. General workshop advice draws on the Wood Handbook; it is not a claim that every operation or application has been tested on this species. Figures above retain the property record’s named sources and licences.

Compare before you choose

See how Red spruce and Black spruce differ in hardness, density, strength, and shrinkage, with sources alongside the values.

Compare Red spruce with Black spruce

Health and safety

A published occupational source reports photosensitisation, respiratory disorders for this wood. What that means, and how strong the link is.

Woods of similar hardness

A substitute must match more than hardness. Compare the shrinkage and the stiffness before you change species.

#WoodJanka
1Black spruce530 lbf
2Gray or California foothill pine532 lbf*
3American chestnut540 lbf
4Guanacaste520 lbf
5Western hemlock540 lbf
6Yellow-poplar540 lbf

All species