Abiurana vs Ingá
Pouteria guianensis against Inga sp. Every number below names the publication it came from.
| Property | Abiurana | Ingá |
|---|---|---|
| Janka hardness | 2,921 lbfLPF/SFB Madeiras Brasileiras | 2,846 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 58.7 lb/ft³LPF/SFB Madeiras Brasileiras | 68.7 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 20,382 lb/in²LPF/SFB Madeiras Brasileiras | 22,915 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | — | 2.25 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 9,871 lb/in²LPF/SFB Madeiras Brasileiras | 11,905 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 13.3%LPF/SFB Madeiras Brasileiras | 12.0%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.76LPF/SFB Madeiras Brasileiras | 2.34LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 3%. Choose on movement or on appearance instead.
- Abiurana moves more evenly. Its tangential-to-radial ratio is 1.8 against 2.3, so it is the safer choice for a wide flat panel.
- Ingá carries 12% more load in bending, which matters for a shelf or a rail.
- Ingá is the heavier of the two by 161 kg/m³, which a reader building a door or a case should weigh.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.