PropertyAbiuranaOak
Janka hardness2,472 lbfLPF/SFB Madeiras Brasileiras2,500 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC56.2 lb/ft³LPF/SFB Madeiras Brasileiras53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture23,525 lb/in²LPF/SFB Madeiras Brasileiras23,000 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity2.31 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras3.02 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength12,246 lb/in²LPF/SFB Madeiras Brasileiras2,960 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)15.2%LPF/SFB Madeiras Brasileiras18.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)1.49LPF/SFB Madeiras Brasileiras1.83USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Abiurana moves more evenly. Its tangential-to-radial ratio is 1.5 against 1.8, so it is the safer choice for a wide flat panel.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons