African Celtis vs African ebony
Celtis spp. against Diospyros spp.. Every number below names the publication it came from.
| Property | African Celtis | African ebony |
|---|---|---|
| Janka hardness | 1,670 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 3,220 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 45.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 63.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 20,900 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 21,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 2.30 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | — |
| Crushing strength | 10,550 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 9,350 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 15.4%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 20.0%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.86Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.17USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- African ebony resists denting better. It tests 93% harder than African Celtis.
- African ebony moves more evenly. Its tangential-to-radial ratio is 1.2 against 1.9, so it is the safer choice for a wide flat panel.
- African ebony is the heavier of the two by 288 kg/m³, which a reader building a door or a case should weigh.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.