Amora / amoreira vs Fustic
Maclura tinctoria against Chlorophora tinctoria. Every number below names the publication it came from.
| Property | Amora / amoreira | Fustic |
|---|---|---|
| Janka hardness | 2,385 lbfLPF/SFB Madeiras Brasileiras | 2,380 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 56.8 lb/ft³LPF/SFB Madeiras Brasileiras | 56.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 22,259 lb/in²LPF/SFB Madeiras Brasileiras | 19,560 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 1.83 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.16 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 12,488 lb/in²LPF/SFB Madeiras Brasileiras | 11,080 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 9.4%LPF/SFB Madeiras Brasileiras | 7.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.84LPF/SFB Madeiras Brasileiras | 1.59Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- The two match on hardness, within 0%. Choose on movement or on appearance instead.
- Fustic moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.8, so it is the safer choice for a wide flat panel.
- Amora / amoreira carries 14% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.