PropertyAngelim / angelim-rajadoPracuúba-da-terra-firme
Janka hardness3,177 lbfLPF/SFB Madeiras Brasileiras3,159 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC61.8 lb/ft³LPF/SFB Madeiras Brasileiras73.4 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture23,724 lb/in²LPF/SFB Madeiras Brasileiras22,871 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.38 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.38 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength11,478 lb/in²LPF/SFB Madeiras Brasileiras12,531 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)15.2%LPF/SFB Madeiras Brasileiras13.2%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.58LPF/SFB Madeiras Brasileiras1.86LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Angelim / angelim-rajado moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.9, so it is the safer choice for a wide flat panel.
  • Pracuúba-da-terra-firme is the heavier of the two by 186 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.