Angelim-vermelho vs Ingá
Dinizia excelsa against Inga paraensis. Every number below names the publication it came from.
| Property | Angelim-vermelho | Ingá |
|---|---|---|
| Janka hardness | 3,045 lbfLPF/SFB Madeiras Brasileiras | 3,064 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 66.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 | 65.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 22,758 lb/in²LPF/SFB Madeiras Brasileiras | 26,540 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.46 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.60 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,417 lb/in²LPF/SFB Madeiras Brasileiras | 12,090 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 14.5%LPF/SFB Madeiras Brasileiras | 15.9%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.67LPF/SFB Madeiras Brasileiras | 2.02LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Angelim-vermelho moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.0, so it is the safer choice for a wide flat panel.
- Ingá carries 17% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.