Anoerá-ferro vs Brazilian rosewood
Acioa sp against Dalbergia nigra. Every number below names the publication it came from.
| Property | Anoerá-ferro | Brazilian rosewood |
|---|---|---|
| Janka hardness | 2,683 lbfLPF/SFB Madeiras Brasileiras | 2,720 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 60.6 lb/ft³LPF/SFB Madeiras Brasileiras | 64.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 20,326 lb/in²LPF/SFB Madeiras Brasileiras | 19,000 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.12 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 1.88 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 10,768 lb/in²LPF/SFB Madeiras Brasileiras | 9,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | 15.1%LPF/SFB Madeiras Brasileiras | 8.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.82LPF/SFB Madeiras Brasileiras | 1.59USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Brazilian rosewood moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.8, so it is the safer choice for a wide flat panel.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.