Azobe vs Caraiperana

Lophira alata against Licania gracilipes. Every number below names the publication it came from.

PropertyAzobeCaraiperana
Janka hardness3,350 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3,294 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)63.7 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture24,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b22,986 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.47 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.35 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength12,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b12,247 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)17.0%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-418.1%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.31USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-42.27LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Azobe moves more evenly. Its tangential-to-radial ratio is 1.3 against 2.3, so it is the safer choice for a wide flat panel.
  • Azobe is the heavier of the two by 101 kg/m³, which a reader building a door or a case should weigh.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.