Azobe vs Rosadinho
Lophira alata against Peltogyne paniculata. Every number below names the publication it came from.
| Property | Azobe | Rosadinho |
|---|---|---|
| Janka hardness | 3,350 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 3,386 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 64.3 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 24,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 27,138 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.47 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2.57 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 13,129 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 17.0%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 12.7%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.31USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.59LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Azobe moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.6, so it is the safer choice for a wide flat panel.
- Rosadinho carries 11% more load in bending, which matters for a shelf or a rail.
- Azobe is the heavier of the two by 91 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.