Barrote vs Leche Perra

Tetragastris panamensis against Helicostylis tomentosa. Every number below names the publication it came from.

PropertyBarroteLeche Perra
Janka hardness2,693 lbfLPF/SFB Madeiras Brasileiras2,700 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC57.4 lb/ft³LPF/SFB Madeiras Brasileiras55.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture17,843 lb/in²LPF/SFB Madeiras Brasileiras22,800 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity1.98 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.86 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength9,373 lb/in²LPF/SFB Madeiras Brasileiras12,300 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)14.9%LPF/SFB Madeiras Brasileiras14.6%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.96LPF/SFB Madeiras Brasileiras1.70Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 0%. Choose on movement or on appearance instead.
  • Leche Perra moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.0, so it is the safer choice for a wide flat panel.
  • Leche Perra carries 28% more load in bending, which matters for a shelf or a rail.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.