PropertyBelianGangaw
Janka hardness3,020 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,890 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC68.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)63.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture25,810 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)24,065 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.65 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)2.87 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength13,620 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)12,430 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)—15.8%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.74Chudnoff 1984, Tropical Timbers of the World (AH-607)1.58Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 4%. Choose on movement or on appearance instead.
  • Belian is the heavier of the two by 80 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons