Eusideroxylon zwageri against Dalbergia latifolia. Every number below names the publication it came from.
| Property | Belian | Indian rosewood |
|---|---|---|
| Janka hardness | 3,020 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 3,170 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 68.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 25,810 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 16,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.65 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.78 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 13,620 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 9,220 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | — | 8.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.74Chudnoff 1984, Tropical Timbers of the World (AH-607) | 2.15USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- Indian rosewood resists denting better. It tests 5% harder than Belian.
- Belian moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.1, so it is the safer choice for a wide flat panel.
- Belian carries 53% more load in bending, which matters for a shelf or a rail.
- Belian is the heavier of the two by 240 kg/m³, which a reader building a door or a case should weigh.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.