Wood Record

Bubinga vs Okan

Guibourtia spp. against Cylicodiscus gabunensis. Every number below names the publication it came from.

PropertyBubingaOkan
Janka hardness2,690 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2,780 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC55.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-964.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture22,600 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b20,300 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.48 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.33 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength10,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b12,380 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)14.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-412.6%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.45USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.47Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 3%. Choose on movement or on appearance instead.
  • Bubinga carries 11% more load in bending, which matters for a shelf or a rail.
  • Okan is the heavier of the two by 131 kg/m³, which a reader building a door or a case should weigh.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons