Wood Record

Bulletwood vs Castanha-de-cutia

Manilkara bidentata against Couepia robusta. Every number below names the publication it came from.

PropertyBulletwoodCastanha-de-cutia
Janka hardness3,190 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3,206 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC66.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)64.3 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture27,300 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b22,416 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity3.45 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b2.26 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength11,640 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b11,436 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)16.9%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-415.7%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.49USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.90LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Bulletwood moves more evenly. Its tangential-to-radial ratio is 1.5 against 1.9, so it is the safer choice for a wide flat panel.
  • Bulletwood carries 22% more load in bending, which matters for a shelf or a rail.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons