Bulletwood vs Pau-santo
Manilkara bidentata against Zollernia paraensis. Every number below names the publication it came from.
| Property | Bulletwood | Pau-santo |
|---|---|---|
| Janka hardness | 3,190 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 3,261 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 66.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 78.7 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 27,300 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 27,238 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 3.45 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2.59 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 11,640 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 13,854 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 16.9%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 16.8%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.49USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.92LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 2%. Choose on movement or on appearance instead.
- Bulletwood moves more evenly. Its tangential-to-radial ratio is 1.5 against 1.9, so it is the safer choice for a wide flat panel.
- Pau-santo is the heavier of the two by 203 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.