Wood Record

Burma Lancewood vs Indian Laurel

Homalium spp. against Terminalia tomentosa complex. Every number below names the publication it came from.

PropertyBurma LancewoodIndian Laurel
Janka hardness2,270 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,220 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC58.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)54.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture15,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)15,380 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.26 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength6,030 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)8,275 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)—13.2%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)—1.54Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons