PropertyBurma PadaukPyinkado
Janka hardness2,170 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,248 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC54.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)61.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture20,640 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)21,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity2.08 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)—
Crushing strength10,945 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)12,300 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)8.4%Chudnoff 1984, Tropical Timbers of the World (AH-607)11.1%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.71Chudnoff 1984, Tropical Timbers of the World (AH-607)2.03Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 4%. Choose on movement or on appearance instead.
  • Burma Padauk moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.0, so it is the safer choice for a wide flat panel.
  • Pyinkado is the heavier of the two by 112 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.