Cabreúva-parda vs Mururé
Myrocarpus frondosus against Brosimum gaudichaudii. Every number below names the publication it came from.
| Property | Cabreúva-parda | Mururé |
|---|---|---|
| Janka hardness | 3,075 lbfLPF/SFB Madeiras Brasileiras | 3,036 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 57.4 lb/ft³LPF/SFB Madeiras Brasileiras | 56.8 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 22,359 lb/in²LPF/SFB Madeiras Brasileiras | 19,941 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.19 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.06 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,460 lb/in²LPF/SFB Madeiras Brasileiras | 11,165 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 11.3%LPF/SFB Madeiras Brasileiras | 14.1%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.59LPF/SFB Madeiras Brasileiras | 1.82LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 1%. Choose on movement or on appearance instead.
- Cabreúva-parda moves more evenly. Its tangential-to-radial ratio is 1.6 against 1.8, so it is the safer choice for a wide flat panel.
- Cabreúva-parda carries 12% more load in bending, which matters for a shelf or a rail.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.