Wood Record

Canafístula vs Pau-branco

Cassia fastuosa against Drypetes variabilis. Every number below names the publication it came from.

PropertyCanafístulaPau-branco
Janka hardness2,500 lbfLPF/SFB Madeiras Brasileiras2,518 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC54.3 lb/ft³LPF/SFB Madeiras Brasileiras55.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture16,527 lb/in²LPF/SFB Madeiras Brasileiras20,865 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity1.91 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.30 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength10,469 lb/in²LPF/SFB Madeiras Brasileiras10,511 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)—15.9%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.47LPF/SFB Madeiras Brasileiras1.95LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Canafístula moves more evenly. Its tangential-to-radial ratio is 1.5 against 1.9, so it is the safer choice for a wide flat panel.
  • Pau-branco carries 26% more load in bending, which matters for a shelf or a rail.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.