PropertyCaraipéMaçarandubarana
Janka hardness2,754 lbfLPF/SFB Madeiras Brasileiras2,725 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC61.3 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-961.8 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture23,355 lb/in²LPF/SFB Madeiras Brasileiras25,232 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.47 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.49 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength12,090 lb/in²LPF/SFB Madeiras Brasileiras10,810 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)17.4%LPF/SFB Madeiras Brasileiras20.3%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.95LPF/SFB Madeiras Brasileiras1.69LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Maçarandubarana moves more evenly. Its tangential-to-radial ratio is 1.7 against 2.0, so it is the safer choice for a wide flat panel.
  • Maçarandubarana carries 8% more load in bending, which matters for a shelf or a rail.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.