PropertyCarne D'AntaFaveira-amargosa
Janka hardness2,240 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,174 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC54.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)62.2 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture18,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)21,519 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.41 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)2.18 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength11,100 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)11,280 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)—14.0%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.93Chudnoff 1984, Tropical Timbers of the World (AH-607)2.04LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 3%. Choose on movement or on appearance instead.
  • Faveira-amargosa carries 18% more load in bending, which matters for a shelf or a rail.
  • Faveira-amargosa is the heavier of the two by 132 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.