Wood Record

Castanha-de-cutia vs Goiabão

Acioa edulis against Chrysophyllum lucentifolium = Pouteria pachycarpa. Every number below names the publication it came from.

PropertyCastanha-de-cutiaGoiabão
Janka hardness2,696 lbfLPF/SFB Madeiras Brasileiras2,646 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC64.9 lb/ft³LPF/SFB Madeiras Brasileiras58.1 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture21,847 lb/in²LPF/SFB Madeiras Brasileiras22,999 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity2.36 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.41 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength11,748 lb/in²LPF/SFB Madeiras Brasileiras11,357 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)17.5%LPF/SFB Madeiras Brasileiras16.5%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.28LPF/SFB Madeiras Brasileiras1.81LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Castanha-de-cutia moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.8, so it is the safer choice for a wide flat panel.
  • Castanha-de-cutia is the heavier of the two by 110 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.