Courbaril vs Greenheart
Hymenaea courbaril against Chlorocardium rodiei. Every number below names the publication it came from.
| Property | Courbaril | Greenheart |
|---|---|---|
| Janka hardness | 2,350 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2,350 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 56.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 64.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 19,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 24,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.16 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 3.25 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 9,510 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 12,510 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | 12.7%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 17.1%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.89USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.09USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- The two match on hardness, within 0%. Choose on movement or on appearance instead.
- Greenheart moves more evenly. Its tangential-to-radial ratio is 1.1 against 1.9, so it is the safer choice for a wide flat panel.
- Greenheart carries 28% more load in bending, which matters for a shelf or a rail.
- Greenheart is the heavier of the two by 130 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- GWDD v2.2 (Fischer et al. 2026)CC BY 4.0
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.