Demerara Greenheart vs Tuturubá

Ocotea rodiaei against Pouteria gongrijpii = Franchetella gongrijpii. Every number below names the publication it came from.

PropertyDemerara GreenheartTuturubá
Janka hardness2,360 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)2,396 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC66.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)56.9 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9
Modulus of rupture26,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)20,951 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity3.04 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)2.22 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength13,040 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)10,952 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)17.1%Chudnoff 1984, Tropical Timbers of the World (AH-607)15.0%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.09Chudnoff 1984, Tropical Timbers of the World (AH-607)2.24LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Demerara Greenheart moves more evenly. Its tangential-to-radial ratio is 1.1 against 2.2, so it is the safer choice for a wide flat panel.
  • Demerara Greenheart carries 25% more load in bending, which matters for a shelf or a rail.
  • Demerara Greenheart is the heavier of the two by 146 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.