East African Olive vs Muhimbi
Olea hochstetteri against Cynometra alexandri. Every number below names the publication it came from.
| Property | East African Olive | Muhimbi |
|---|---|---|
| Janka hardness | 2,740 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,975 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 55.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 54.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 25,300 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 21,900 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 2.53 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 2.05 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 12,200 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 10,400 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | — | — |
| Tangential / radial ratio(lower is better) | — | — |
What the numbers mean
- Muhimbi resists denting better. It tests 9% harder than East African Olive.
- East African Olive carries 16% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.