East Indian ebony vs East Indian Satinwood
Diospyros spp. against Chloroxylon swietenia. Every number below names the publication it came from.
| Property | East Indian ebony | East Indian Satinwood |
|---|---|---|
| Janka hardness | 1,630 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,600 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 52.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 61.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 11,125 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 16,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 1.44 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 2.02 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 5,960 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 10,030 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 14.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | — |
| Tangential / radial ratio(lower is better) | 1.63USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.29Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- East Indian Satinwood resists denting better. It tests 60% harder than East Indian ebony.
- East Indian Satinwood moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.6, so it is the safer choice for a wide flat panel.
- East Indian Satinwood carries 48% more load in bending, which matters for a shelf or a rail.
- East Indian Satinwood is the heavier of the two by 144 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.