Wood Record

East Indian ebony vs Indian rosewood

Diospyros spp. against Dalbergia latifolia. Every number below names the publication it came from.

PropertyEast Indian ebonyIndian rosewood
Janka hardness1,630 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)3,170 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC52.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture11,125 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)16,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity1.44 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.78 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength5,960 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)9,220 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)14.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-48.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)1.63USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-42.15USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • Indian rosewood resists denting better. It tests 94% harder than East Indian ebony.
  • East Indian ebony moves more evenly. Its tangential-to-radial ratio is 1.6 against 2.1, so it is the safer choice for a wide flat panel.
  • Indian rosewood carries 52% more load in bending, which matters for a shelf or a rail.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons