East Indian Satinwood vs Gangaw
Chloroxylon swietenia against Mesua ferrea. Every number below names the publication it came from.
| Property | East Indian Satinwood | Gangaw |
|---|---|---|
| Janka hardness | 2,600 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,890 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 61.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 63.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 16,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 24,065 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 2.02 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 2.87 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 10,030 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 12,430 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | — | 15.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.29Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.58Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- Gangaw resists denting better. It tests 11% harder than East Indian Satinwood.
- East Indian Satinwood moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.6, so it is the safer choice for a wide flat panel.
- Gangaw carries 46% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.