Chloroxylon swietenia against Dalbergia latifolia. Every number below names the publication it came from.

PropertyEast Indian SatinwoodIndian rosewood
Janka hardness2,600 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)3,170 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC61.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)53.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture16,500 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)16,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity2.02 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)1.78 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength10,030 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)9,220 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)—8.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)1.29Chudnoff 1984, Tropical Timbers of the World (AH-607)2.15USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • Indian rosewood resists denting better. It tests 22% harder than East Indian Satinwood.
  • East Indian Satinwood moves more evenly. Its tangential-to-radial ratio is 1.3 against 2.1, so it is the safer choice for a wide flat panel.
  • East Indian Satinwood is the heavier of the two by 128 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.