Faveira-amargosa vs Tanimbuca
Vatairea paraensis against Terminalia amazonia. Every number below names the publication it came from.
| Property | Faveira-amargosa | Tanimbuca |
|---|---|---|
| Janka hardness | 2,174 lbfLPF/SFB Madeiras Brasileiras | 2,235 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 62.2 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 | 64.1 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9 |
| Modulus of rupture | 21,519 lb/in²LPF/SFB Madeiras Brasileiras | 21,178 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.18 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras | 2.03 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 11,280 lb/in²LPF/SFB Madeiras Brasileiras | 11,307 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 14.0%LPF/SFB Madeiras Brasileiras | 12.8%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 2.04LPF/SFB Madeiras Brasileiras | 1.50LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 3%. Choose on movement or on appearance instead.
- Tanimbuca moves more evenly. Its tangential-to-radial ratio is 1.5 against 2.0, so it is the safer choice for a wide flat panel.
Sources
- LPF/SFB Madeiras BrasileirasCC BY 4.0
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.