Gangaw vs Kaneelhart
Mesua ferrea against Licaria spp.. Every number below names the publication it came from.
| Property | Gangaw | Kaneelhart |
|---|---|---|
| Janka hardness | 2,890 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 2,900 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 63.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 24,065 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 29,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.87 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 4.06 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 12,430 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 17,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | 15.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 12.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.58Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.46USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- The two match on hardness, within 0%. Choose on movement or on appearance instead.
- Kaneelhart carries 24% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.