Wood Record

Ingá vs Kaneelhart

Inga sp against Licaria spp.. Every number below names the publication it came from.

PropertyIngáKaneelhart
Janka hardness2,846 lbfLPF/SFB Madeiras Brasileiras2,900 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC68.7 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-962.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture22,915 lb/in²LPF/SFB Madeiras Brasileiras29,900 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity2.25 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras4.06 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength11,905 lb/in²LPF/SFB Madeiras Brasileiras17,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)12.0%LPF/SFB Madeiras Brasileiras12.5%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)2.34LPF/SFB Madeiras Brasileiras1.46USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Kaneelhart moves more evenly. Its tangential-to-radial ratio is 1.5 against 2.3, so it is the safer choice for a wide flat panel.
  • Kaneelhart carries 30% more load in bending, which matters for a shelf or a rail.
  • Ingá is the heavier of the two by 108 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons