Wood Record

Ipê vs Maçaranduba

Handroanthus serratifolius = Tabebuia serratifolia against Manilkara huberi. Every number below names the publication it came from.

PropertyIpêMaçaranduba
Janka hardness3,100 lbfLPF/SFB Madeiras Brasileiras3,047 lbfLPF/SFB Madeiras Brasileiras
Density at 12% MC72.5 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-966.8 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture24,549 lb/in²LPF/SFB Madeiras Brasileiras25,560 lb/in²LPF/SFB Madeiras Brasileiras
Modulus of elasticity1.86 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras2.47 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras
Crushing strength12,360 lb/in²LPF/SFB Madeiras Brasileiras15,774 lb/in²LPF/SFB Madeiras Brasileiras
Volumetric shrinkage(lower is better)10.1%LPF/SFB Madeiras Brasileiras16.4%LPF/SFB Madeiras Brasileiras
Tangential / radial ratio(lower is better)1.34LPF/SFB Madeiras Brasileiras1.31LPF/SFB Madeiras Brasileiras

What the numbers mean

  • The two match on hardness, within 2%. Choose on movement or on appearance instead.
  • Ipê is the heavier of the two by 91 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons