Wood Record

Ipê vs Sapucaia

Handroanthus serratifolius = Tabebuia serratifolia against Lecythis spp.. Every number below names the publication it came from.

PropertyIpêSapucaia
Janka hardness3,100 lbfLPF/SFB Madeiras Brasileiras3,100 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)
Density at 12% MC72.5 lb/ft³EstimateUSDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-958.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture24,549 lb/in²LPF/SFB Madeiras Brasileiras27,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of elasticity1.86 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras3.38 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Crushing strength12,360 lb/in²LPF/SFB Madeiras Brasileiras13,280 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)
Volumetric shrinkage(lower is better)10.1%LPF/SFB Madeiras Brasileiras13.4%Chudnoff 1984, Tropical Timbers of the World (AH-607)
Tangential / radial ratio(lower is better)1.34LPF/SFB Madeiras Brasileiras1.27Chudnoff 1984, Tropical Timbers of the World (AH-607)

What the numbers mean

  • The two match on hardness, within 0%. Choose on movement or on appearance instead.
  • Sapucaia carries 12% more load in bending, which matters for a shelf or a rail.
  • Ipê is the heavier of the two by 232 kg/m³, which a reader building a door or a case should weigh.

Sources

  • LPF/SFB Madeiras BrasileirasCC BY 4.0
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons