Ipe vs Jarana
Tabebuia spp., lapacho group against Holopyxidium jarana. Every number below names the publication it came from.
| Property | Ipe | Jarana |
|---|---|---|
| Janka hardness | 3,680 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 3,500 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 25,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 30,170 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 3.14 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 2.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 13,010 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b | 12,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 13.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 16.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.21USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 | 1.34Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- Ipe resists denting better. It tests 5% harder than Jarana.
- Jarana carries 19% more load in bending, which matters for a shelf or a rail.
- Ipe is the heavier of the two by 128 kg/m³, which a reader building a door or a case should weigh.
Sources
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.