Wood Record

Ipe vs Marishballi

Tabebuia spp., lapacho group against Lincania spp.. Every number below names the publication it came from.

PropertyIpeMarishballi
Janka hardness3,680 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3,570 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)
Modulus of rupture25,400 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b27,700 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity3.14 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b3.34 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength13,010 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b13,390 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)13.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-417.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)1.21USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-41.56USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • The two match on hardness, within 3%. Choose on movement or on appearance instead.
  • Ipe moves more evenly. Its tangential-to-radial ratio is 1.2 against 1.6, so it is the safer choice for a wide flat panel.
  • Marishballi carries 9% more load in bending, which matters for a shelf or a rail.
  • Ipe is the heavier of the two by 128 kg/m³, which a reader building a door or a case should weigh.

Sources

  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.

All comparisons