Jarana vs Jataipeba
Holopyxidium jarana against Dialium guianense. Every number below names the publication it came from.
| Property | Jarana | Jataipeba |
|---|---|---|
| Janka hardness | 3,500 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 3,650 lbfLPF/SFB Madeiras Brasileiras |
| Density at 12% MC | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 63.7 lb/ft³LPF/SFB Madeiras Brasileiras |
| Modulus of rupture | 30,170 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 24,614 lb/in²LPF/SFB Madeiras Brasileiras |
| Modulus of elasticity | 2.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 2.35 ×10⁶ lb/in²LPF/SFB Madeiras Brasileiras |
| Crushing strength | 12,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 12,481 lb/in²LPF/SFB Madeiras Brasileiras |
| Volumetric shrinkage(lower is better) | 16.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 14.5%LPF/SFB Madeiras Brasileiras |
| Tangential / radial ratio(lower is better) | 1.34Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.75LPF/SFB Madeiras Brasileiras |
What the numbers mean
- The two match on hardness, within 4%. Choose on movement or on appearance instead.
- Jarana moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.7, so it is the safer choice for a wide flat panel.
- Jarana carries 23% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- LPF/SFB Madeiras BrasileirasCC BY 4.0
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.