PropertyJaranaManbarklak
Janka hardness3,500 lbfChudnoff 1984, Tropical Timbers of the World (AH-607)3,480 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Density at 12% MC62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607)46.2 lb/ft³LPF/SFB Madeiras Brasileiras
Modulus of rupture30,170 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)26,500 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Modulus of elasticity2.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)3.14 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Crushing strength12,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607)11,210 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b
Volumetric shrinkage(lower is better)16.8%Chudnoff 1984, Tropical Timbers of the World (AH-607)15.9%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4
Tangential / radial ratio(lower is better)1.34Chudnoff 1984, Tropical Timbers of the World (AH-607)1.78USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4

What the numbers mean

  • The two match on hardness, within 1%. Choose on movement or on appearance instead.
  • Jarana moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.8, so it is the safer choice for a wide flat panel.
  • Jarana carries 14% more load in bending, which matters for a shelf or a rail.
  • Jarana is the heavier of the two by 253 kg/m³, which a reader building a door or a case should weigh.

Sources

  • Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
  • USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
  • LPF/SFB Madeiras BrasileirasCC BY 4.0

Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.