Jarana vs Marishballi
Holopyxidium jarana against Lincania spp.. Every number below names the publication it came from.
| Property | Jarana | Marishballi |
|---|---|---|
| Janka hardness | 3,500 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 3,570 lbfUSDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Density at 12% MC | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 30,170 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 27,700 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Modulus of elasticity | 2.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 3.34 ×10⁶ lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Crushing strength | 12,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 13,390 lb/in²USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5b |
| Volumetric shrinkage(lower is better) | 16.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 17.2%USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
| Tangential / radial ratio(lower is better) | 1.34Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.56USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4 |
What the numbers mean
- The two match on hardness, within 2%. Choose on movement or on appearance instead.
- Jarana moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.6, so it is the safer choice for a wide flat panel.
- Jarana carries 9% more load in bending, which matters for a shelf or a rail.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 5-5bpublic domain
- USDA Wood Handbook 2021 (FPL-GTR-282) Table 4-4public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.