Jarana vs Wamara
Holopyxidium jarana against Swartzia spp.. Every number below names the publication it came from.
| Property | Jarana | Wamara |
|---|---|---|
| Janka hardness | 3,500 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) | 3,692 lbfChudnoff 1984, Tropical Timbers of the World (AH-607) |
| Density at 12% MC | 62.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) | 70.0 lb/ft³Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of rupture | 30,170 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 26,370 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Modulus of elasticity | 2.91 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 3.63 ×10⁶ lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Crushing strength | 12,540 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) | 15,440 lb/in²Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Volumetric shrinkage(lower is better) | 16.8%Chudnoff 1984, Tropical Timbers of the World (AH-607) | 11.2%Chudnoff 1984, Tropical Timbers of the World (AH-607) |
| Tangential / radial ratio(lower is better) | 1.34Chudnoff 1984, Tropical Timbers of the World (AH-607) | 1.95Chudnoff 1984, Tropical Timbers of the World (AH-607) |
What the numbers mean
- Wamara resists denting better. It tests 5% harder than Jarana.
- Jarana moves more evenly. Its tangential-to-radial ratio is 1.3 against 1.9, so it is the safer choice for a wide flat panel.
- Jarana carries 14% more load in bending, which matters for a shelf or a rail.
- Wamara is the heavier of the two by 128 kg/m³, which a reader building a door or a case should weigh.
Sources
- Chudnoff 1984, Tropical Timbers of the World (AH-607)public domain
- USDA Wood Handbook 2021 (FPL-GTR-282) eq. 4-9public domain
Estimates are labeled beside their values. A dash means no published value is available. Properties describe the source material; individual boards vary.